Physical Properties | Metric | English | Comments |
---|
Density | 7.65 g/cc | 0.276 lb/in³ |
Thickness | 270 - 310 microns | 10.6 - 12.2 mil |
| 300 microns | 11.8 mil |
|
Mechanical Properties | Metric | English | Comments |
---|
Knoop Microhardness | 173 | 173 |
Hardness, Rockwell B | 83 | 83 |
Tensile Strength, Ultimate | 359 MPa | 52100 psi |
Tensile Strength, Yield | 345 MPa | 50000 psi |
Elongation at Break | 11 % | 11 % |
Modulus of Elasticity | 113.8 GPa | 16510 ksi |
| 138 GPa | 20000 ksi |
| 203 GPa | 29400 ksi |
| 241 GPa | 35000 ksi |
| 276 GPa | 40000 ksi |
|
Electrical Properties | Metric | English | Comments |
---|
Exciting Power (RMS) | 0.00196 RMS AT/cm @Magnetic Field 0.100 T, Frequency 50 Hz | 0.00310 RMS VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00215 RMS AT/cm @Magnetic Field 0.100 T, Frequency 50 Hz | 0.00340 RMS VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00253 RMS AT/cm @Magnetic Field 0.100 T, Frequency 60 Hz | 0.00400 RMS VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00272 RMS AT/cm @Magnetic Field 0.100 T, Frequency 60 Hz | 0.00430 RMS VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00696 RMS AT/cm @Magnetic Field 0.200 T, Frequency 50 Hz | 0.0110 RMS VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.00721 RMS AT/cm @Magnetic Field 0.200 T, Frequency 50 Hz | 0.0114 RMS VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.00892 RMS AT/cm @Magnetic Field 0.200 T, Frequency 60 Hz | 0.0141 RMS VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.00930 RMS AT/cm @Magnetic Field 0.200 T, Frequency 60 Hz | 0.0147 RMS VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0144 RMS AT/cm @Magnetic Field 0.300 T, Frequency 50 Hz | 0.0228 RMS VA/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0147 RMS AT/cm @Magnetic Field 0.300 T, Frequency 50 Hz | 0.0233 RMS VA/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0186 RMS AT/cm @Magnetic Field 0.300 T, Frequency 60 Hz | 0.0294 RMS VA/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0190 RMS AT/cm @Magnetic Field 0.300 T, Frequency 60 Hz | 0.0300 RMS VA/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0239 RMS AT/cm @Magnetic Field 0.400 T, Frequency 50 Hz | 0.0378 RMS VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0241 RMS AT/cm @Magnetic Field 0.400 T, Frequency 50 Hz | 0.0381 RMS VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0309 RMS AT/cm @Magnetic Field 0.400 T, Frequency 60 Hz | 0.0488 RMS VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0311 RMS AT/cm @Magnetic Field 0.400 T, Frequency 60 Hz | 0.0492 RMS VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0351 RMS AT/cm @Magnetic Field 0.500 T, Frequency 50 Hz | 0.0554 RMS VA/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0352 RMS AT/cm @Magnetic Field 0.500 T, Frequency 50 Hz | 0.0556 RMS VA/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0454 RMS AT/cm @Magnetic Field 0.500 T, Frequency 60 Hz | 0.0717 RMS VA/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0456 RMS AT/cm @Magnetic Field 0.500 T, Frequency 60 Hz | 0.0720 RMS VA/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0478 RMS AT/cm @Magnetic Field 0.600 T, Frequency 50 Hz | 0.0755 RMS VA/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0478 RMS AT/cm @Magnetic Field 0.600 T, Frequency 50 Hz | 0.0755 RMS VA/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0618 RMS AT/cm @Magnetic Field 0.600 T, Frequency 60 Hz | 0.0977 RMS VA/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.0618 RMS AT/cm @Magnetic Field 0.700 T, Frequency 50 Hz | 0.0977 RMS VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.0618 RMS AT/cm @Magnetic Field 0.600 T, Frequency 60 Hz | 0.0977 RMS VA/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.0618 RMS AT/cm @Magnetic Field 0.700 T, Frequency 50 Hz | 0.0977 RMS VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.07738 RMS AT/cm @Magnetic Field 0.800 T, Frequency 50 Hz | 0.1223 RMS VA/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.07763 RMS AT/cm @Magnetic Field 0.800 T, Frequency 50 Hz | 0.1227 RMS VA/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.08023 RMS AT/cm @Magnetic Field 0.700 T, Frequency 60 Hz | 0.1268 RMS VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.08054 RMS AT/cm @Magnetic Field 0.700 T, Frequency 60 Hz | 0.1273 RMS VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.09434 RMS AT/cm @Magnetic Field 0.900 T, Frequency 50 Hz | 0.1491 RMS VA/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.0949 RMS AT/cm @Magnetic Field 0.900 T, Frequency 50 Hz | 0.150 RMS VA/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.1007 RMS AT/cm @Magnetic Field 0.800 T, Frequency 60 Hz | 0.1591 RMS VA/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.101 RMS AT/cm @Magnetic Field 0.800 T, Frequency 60 Hz | 0.160 RMS VA/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.1133 RMS AT/cm @Magnetic Field 1.00 T, Frequency 50 Hz | 0.1791 RMS VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.114 RMS AT/cm @Magnetic Field 1.00 T, Frequency 50 Hz | 0.180 RMS VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.123 RMS AT/cm @Magnetic Field 0.900 T, Frequency 60 Hz | 0.195 RMS VA/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.1239 RMS AT/cm @Magnetic Field 0.900 T, Frequency 60 Hz | 0.1959 RMS VA/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.1338 RMS AT/cm @Magnetic Field 1.10 T, Frequency 50 Hz | 0.2114 RMS VA/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.1349 RMS AT/cm @Magnetic Field 1.10 T, Frequency 50 Hz | 0.2132 RMS VA/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.1481 RMS AT/cm @Magnetic Field 1.00 T, Frequency 60 Hz | 0.2341 RMS VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.1490 RMS AT/cm @Magnetic Field 1.00 T, Frequency 60 Hz | 0.2355 RMS VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.1565 RMS AT/cm @Magnetic Field 1.20 T, Frequency 50 Hz | 0.2473 RMS VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.1579 RMS AT/cm @Magnetic Field 1.20 T, Frequency 50 Hz | 0.2495 RMS VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.1751 RMS AT/cm @Magnetic Field 1.10 T, Frequency 60 Hz | 0.2768 RMS VA/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.1766 RMS AT/cm @Magnetic Field 1.10 T, Frequency 60 Hz | 0.2791 RMS VA/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.1820 RMS AT/cm @Magnetic Field 1.30 T, Frequency 50 Hz | 0.2877 RMS VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.183 RMS AT/cm @Magnetic Field 1.30 T, Frequency 50 Hz | 0.290 RMS VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.2051 RMS AT/cm @Magnetic Field 1.20 T, Frequency 60 Hz | 0.3241 RMS VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.2071 RMS AT/cm @Magnetic Field 1.20 T, Frequency 60 Hz | 0.3273 RMS VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.2105 RMS AT/cm @Magnetic Field 1.40 T, Frequency 50 Hz | 0.3327 RMS VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.2131 RMS AT/cm @Magnetic Field 1.40 T, Frequency 50 Hz | 0.3368 RMS VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.2387 RMS AT/cm @Magnetic Field 1.30 T, Frequency 60 Hz | 0.3773 RMS VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.2407 RMS AT/cm @Magnetic Field 1.30 T, Frequency 60 Hz | 0.3805 RMS VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.2462 RMS AT/cm @Magnetic Field 1.50 T, Frequency 50 Hz | 0.3891 RMS VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.2493 RMS AT/cm @Magnetic Field 1.50 T, Frequency 50 Hz | 0.3941 RMS VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.2761 RMS AT/cm @Magnetic Field 1.40 T, Frequency 60 Hz | 0.4364 RMS VA/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.2795 RMS AT/cm @Magnetic Field 1.40 T, Frequency 60 Hz | 0.4418 RMS VA/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.2945 RMS AT/cm @Magnetic Field 1.60 T, Frequency 50 Hz | 0.4655 RMS VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.2988 RMS AT/cm @Magnetic Field 1.60 T, Frequency 50 Hz | 0.4723 RMS VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.3221 RMS AT/cm @Magnetic Field 1.50 T, Frequency 60 Hz | 0.5091 RMS VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.3262 RMS AT/cm @Magnetic Field 1.50 T, Frequency 60 Hz | 0.5155 RMS VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.3770 RMS AT/cm @Magnetic Field 1.70 T, Frequency 50 Hz | 0.5959 RMS VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.3822 RMS AT/cm @Magnetic Field 1.70 T, Frequency 50 Hz | 0.6041 RMS VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.383 RMS AT/cm @Magnetic Field 1.60 T, Frequency 60 Hz | 0.605 RMS VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.3885 RMS AT/cm @Magnetic Field 1.60 T, Frequency 60 Hz | 0.6141 RMS VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.484 RMS AT/cm @Magnetic Field 1.70 T, Frequency 60 Hz | 0.765 RMS VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 0.4907 RMS AT/cm @Magnetic Field 1.70 T, Frequency 60 Hz | 0.7755 RMS VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 0.6241 RMS AT/cm @Magnetic Field 1.80 T, Frequency 50 Hz | 0.9864 RMS VA/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 0.6241 RMS AT/cm @Magnetic Field 1.80 T, Frequency 50 Hz | 0.9864 RMS VA/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 0.77936 RMS AT/cm @Magnetic Field 1.80 T, Frequency 60 Hz | 1.2318 RMS VA/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 0.77936 RMS AT/cm @Magnetic Field 1.80 T, Frequency 60 Hz | 1.2318 RMS VA/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 2.6918 RMS AT/cm @Magnetic Field 1.90 T, Frequency 50 Hz | 4.2545 RMS VA/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 2.6976 RMS AT/cm @Magnetic Field 1.90 T, Frequency 50 Hz | 4.2636 RMS VA/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 3.3418 RMS AT/cm @Magnetic Field 1.90 T, Frequency 60 Hz | 5.2818 RMS VA/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
| 3.3418 RMS AT/cm @Magnetic Field 1.90 T, Frequency 60 Hz | 5.2818 RMS VA/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
Electrical Resistivity | 0.0000500 ohm-cm | 0.0000500 ohm-cm |
|
Magnetic Properties | Metric | English | Comments |
---|
Core Loss | 0.00423 W/kg @Magnetic Field 0.100 T, Frequency 50 Hz | 0.00192 W/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00436 W/kg @Magnetic Field 0.100 T, Frequency 50 Hz | 0.00198 W/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00569 W/kg @Magnetic Field 0.100 T, Frequency 60 Hz | 0.00258 W/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00586 W/kg @Magnetic Field 0.100 T, Frequency 60 Hz | 0.00266 W/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.01586 W/kg @Magnetic Field 0.200 T, Frequency 50 Hz | 0.007194 W/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.01613 W/kg @Magnetic Field 0.200 T, Frequency 50 Hz | 0.007316 W/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0214 W/kg @Magnetic Field 0.200 T, Frequency 60 Hz | 0.00971 W/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0218 W/kg @Magnetic Field 0.200 T, Frequency 60 Hz | 0.00989 W/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0343 W/kg @Magnetic Field 0.300 T, Frequency 50 Hz | 0.0156 W/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0350 W/kg @Magnetic Field 0.300 T, Frequency 50 Hz | 0.0159 W/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0372 W/kg @Magnetic Field 0.500 T, Frequency 50 Hz | 0.0169 W/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0463 W/kg @Magnetic Field 0.300 T, Frequency 60 Hz | 0.0210 W/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0472 W/kg @Magnetic Field 0.300 T, Frequency 60 Hz | 0.0214 W/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0593 W/kg @Magnetic Field 0.400 T, Frequency 50 Hz | 0.0269 W/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0603 W/kg @Magnetic Field 0.400 T, Frequency 50 Hz | 0.0274 W/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0799 W/kg @Magnetic Field 0.400 T, Frequency 60 Hz | 0.0362 W/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0812 W/kg @Magnetic Field 0.400 T, Frequency 60 Hz | 0.0368 W/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0917 W/kg @Magnetic Field 0.500 T, Frequency 50 Hz | 0.0416 W/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.1211 W/kg @Magnetic Field 0.500 T, Frequency 60 Hz | 0.05493 W/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.1232 W/kg @Magnetic Field 0.500 T, Frequency 60 Hz | 0.05588 W/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.1267 W/kg @Magnetic Field 0.600 T, Frequency 50 Hz | 0.05747 W/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.1288 W/kg @Magnetic Field 0.600 T, Frequency 50 Hz | 0.05842 W/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.1687 W/kg @Magnetic Field 0.700 T, Frequency 50 Hz | 0.07652 W/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.1699 W/kg @Magnetic Field 0.600 T, Frequency 60 Hz | 0.07707 W/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.1717 W/kg @Magnetic Field 0.700 T, Frequency 50 Hz | 0.07788 W/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.1727 W/kg @Magnetic Field 0.600 T, Frequency 60 Hz | 0.07834 W/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.216 W/kg @Magnetic Field 0.800 T, Frequency 50 Hz | 0.0980 W/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.220 W/kg @Magnetic Field 0.800 T, Frequency 50 Hz | 0.0998 W/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.226 W/kg @Magnetic Field 0.700 T, Frequency 60 Hz | 0.103 W/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.230 W/kg @Magnetic Field 0.700 T, Frequency 60 Hz | 0.104 W/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.269 W/kg @Magnetic Field 0.900 T, Frequency 50 Hz | 0.122 W/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.275 W/kg @Magnetic Field 0.900 T, Frequency 50 Hz | 0.125 W/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.289 W/kg @Magnetic Field 0.800 T, Frequency 60 Hz | 0.131 W/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.295 W/kg @Magnetic Field 0.800 T, Frequency 60 Hz | 0.134 W/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.329 W/kg @Magnetic Field 1.00 T, Frequency 50 Hz | 0.149 W/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.337 W/kg @Magnetic Field 1.00 T, Frequency 50 Hz | 0.153 W/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.360 W/kg @Magnetic Field 0.900 T, Frequency 60 Hz | 0.163 W/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.368 W/kg @Magnetic Field 0.900 T, Frequency 60 Hz | 0.167 W/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.395 W/kg @Magnetic Field 1.10 T, Frequency 50 Hz | 0.179 W/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.405 W/kg @Magnetic Field 1.10 T, Frequency 50 Hz | 0.184 W/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.439 W/kg @Magnetic Field 1.00 T, Frequency 60 Hz | 0.199 W/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.450 W/kg @Magnetic Field 1.00 T, Frequency 60 Hz | 0.204 W/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.468 W/kg @Magnetic Field 1.20 T, Frequency 50 Hz | 0.212 W/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.479 W/kg @Magnetic Field 1.20 T, Frequency 50 Hz | 0.217 W/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.527 W/kg @Magnetic Field 1.10 T, Frequency 60 Hz | 0.239 W/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.540 W/kg @Magnetic Field 1.10 T, Frequency 60 Hz | 0.245 W/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.548 W/kg @Magnetic Field 1.30 T, Frequency 50 Hz | 0.249 W/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.561 W/kg @Magnetic Field 1.30 T, Frequency 50 Hz | 0.254 W/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.625 W/kg @Magnetic Field 1.20 T, Frequency 60 Hz | 0.283 W/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.636 W/kg @Magnetic Field 1.40 T, Frequency 50 Hz | 0.288 W/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.640 W/kg @Magnetic Field 1.20 T, Frequency 60 Hz | 0.290 W/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.650 W/kg @Magnetic Field 1.40 T, Frequency 50 Hz | 0.295 W/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.732 W/kg @Magnetic Field 1.30 T, Frequency 60 Hz | 0.332 W/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.737 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz | 0.334 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.740 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz | 0.336 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.748 W/kg @Magnetic Field 1.30 T, Frequency 60 Hz | 0.339 W/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.750 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz | 0.340 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.846 W/kg @Magnetic Field 1.60 T, Frequency 50 Hz | 0.384 W/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.849 W/kg @Magnetic Field 1.40 T, Frequency 60 Hz | 0.385 W/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.864 W/kg @Magnetic Field 1.60 T, Frequency 50 Hz | 0.392 W/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.868 W/kg @Magnetic Field 1.40 T, Frequency 60 Hz | 0.394 W/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.980 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz | 0.445 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.982 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz | 0.445 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.990 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | 0.449 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.992 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | 0.450 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.999 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz | 0.453 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 1.007 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | 0.4568 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 1.05 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | 0.476 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 1.126 W/kg @Magnetic Field 1.60 T, Frequency 60 Hz | 0.5107 W/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 1.149 W/kg @Magnetic Field 1.60 T, Frequency 60 Hz | 0.5212 W/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 1.222 W/kg @Magnetic Field 1.80 T, Frequency 50 Hz | 0.5543 W/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 1.245 W/kg @Magnetic Field 1.80 T, Frequency 50 Hz | 0.5647 W/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 1.31 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | 0.594 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.313 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | 0.5956 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.333 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | 0.6046 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.40 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | 0.635 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.596 W/kg @Magnetic Field 1.80 T, Frequency 60 Hz | 0.7239 W/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 1.629 W/kg @Magnetic Field 1.80 T, Frequency 60 Hz | 0.7389 W/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 1.718 W/kg @Magnetic Field 1.90 T, Frequency 50 Hz | 0.7793 W/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 1.746 W/kg @Magnetic Field 1.90 T, Frequency 50 Hz | 0.7920 W/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 2.22 W/kg @Magnetic Field 1.90 T, Frequency 60 Hz | 1.01 W/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
| 2.26 W/kg @Magnetic Field 1.90 T, Frequency 60 Hz | 1.03 W/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
|
Descriptive Properties |
---|
Approximate Equivalent International Grade | M105-30P5 |
Magnetostriction 10^8 | -45 |
| -48 |
| -53 |
| -55 |
Maximum Induction at 800 A/m (T) | 1.9 |
Minimum Lamination Factor (%) | 95.5 |
Typical Induction at 800 A/m (T) | 1.92 |