Physical Properties | Metric | English | Comments |
---|
Density | 7.65 g/cc | 0.276 lb/in³ |
Thickness | 305 microns | 12.0 mil |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Knoop | 167 | 167 |
Hardness, Rockwell B | 81 | 81 |
Tensile Strength, Ultimate | 352 MPa | 51000 psi |
Tensile Strength, Yield | 331 MPa | 48000 psi |
Elongation at Break | 9.0 % | 9.0 % |
Modulus of Elasticity | 122 GPa | 17700 ksi |
| 143 GPa | 20700 ksi |
| 200 GPa | 29000 ksi |
| 236 GPa | 34200 ksi |
| 258 GPa | 37400 ksi |
|
Electrical Properties | Metric | English | Comments |
---|
Exciting Power (RMS) | 0.00252 RMS AT/cm @Magnetic Field 0.100 T, Frequency 50 Hz | 0.00398 RMS VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00264 RMS AT/cm @Magnetic Field 0.100 T, Frequency 50 Hz | 0.00418 RMS VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00314 RMS AT/cm @Magnetic Field 0.100 T, Frequency 60 Hz | 0.00496 RMS VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00330 RMS AT/cm @Magnetic Field 0.100 T, Frequency 60 Hz | 0.00521 RMS VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00854 RMS AT/cm @Magnetic Field 0.200 T, Frequency 50 Hz | 0.0135 RMS VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.00873 RMS AT/cm @Magnetic Field 0.200 T, Frequency 50 Hz | 0.0138 RMS VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0108 RMS AT/cm @Magnetic Field 0.200 T, Frequency 60 Hz | 0.0171 RMS VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0110 RMS AT/cm @Magnetic Field 0.200 T, Frequency 60 Hz | 0.0174 RMS VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0173 RMS AT/cm @Magnetic Field 0.300 T, Frequency 50 Hz | 0.0274 RMS VA/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0174 RMS AT/cm @Magnetic Field 0.300 T, Frequency 50 Hz | 0.0275 RMS VA/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0220 RMS AT/cm @Magnetic Field 0.300 T, Frequency 60 Hz | 0.0347 RMS VA/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0220 RMS AT/cm @Magnetic Field 0.300 T, Frequency 60 Hz | 0.0348 RMS VA/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0283 RMS AT/cm @Magnetic Field 0.400 T, Frequency 50 Hz | 0.0447 RMS VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0283 RMS AT/cm @Magnetic Field 0.400 T, Frequency 50 Hz | 0.0448 RMS VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0359 RMS AT/cm @Magnetic Field 0.400 T, Frequency 60 Hz | 0.0567 RMS VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0360 RMS AT/cm @Magnetic Field 0.400 T, Frequency 60 Hz | 0.0569 RMS VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0411 RMS AT/cm @Magnetic Field 0.500 T, Frequency 50 Hz | 0.0650 RMS VA/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0413 RMS AT/cm @Magnetic Field 0.500 T, Frequency 50 Hz | 0.0652 RMS VA/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0523 RMS AT/cm @Magnetic Field 0.500 T, Frequency 60 Hz | 0.0827 RMS VA/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0526 RMS AT/cm @Magnetic Field 0.500 T, Frequency 60 Hz | 0.0831 RMS VA/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0558 RMS AT/cm @Magnetic Field 0.600 T, Frequency 50 Hz | 0.0882 RMS VA/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0561 RMS AT/cm @Magnetic Field 0.600 T, Frequency 50 Hz | 0.0887 RMS VA/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0709 RMS AT/cm @Magnetic Field 0.600 T, Frequency 60 Hz | 0.112 RMS VA/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.0715 RMS AT/cm @Magnetic Field 0.600 T, Frequency 60 Hz | 0.113 RMS VA/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.0721 RMS AT/cm @Magnetic Field 0.700 T, Frequency 50 Hz | 0.114 RMS VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.0728 RMS AT/cm @Magnetic Field 0.700 T, Frequency 50 Hz | 0.115 RMS VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.0911 RMS AT/cm @Magnetic Field 0.800 T, Frequency 50 Hz | 0.144 RMS VA/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.0917 RMS AT/cm @Magnetic Field 0.800 T, Frequency 50 Hz | 0.145 RMS VA/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.0930 RMS AT/cm @Magnetic Field 0.700 T, Frequency 60 Hz | 0.147 RMS VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.0930 RMS AT/cm @Magnetic Field 0.700 T, Frequency 60 Hz | 0.147 RMS VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.112 RMS AT/cm @Magnetic Field 0.900 T, Frequency 50 Hz | 0.177 RMS VA/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.113 RMS AT/cm @Magnetic Field 0.900 T, Frequency 50 Hz | 0.178 RMS VA/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.117 RMS AT/cm @Magnetic Field 0.800 T, Frequency 60 Hz | 0.185 RMS VA/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.118 RMS AT/cm @Magnetic Field 0.800 T, Frequency 60 Hz | 0.186 RMS VA/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.136 RMS AT/cm @Magnetic Field 1.00 T, Frequency 50 Hz | 0.215 RMS VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.136 RMS AT/cm @Magnetic Field 1.00 T, Frequency 50 Hz | 0.215 RMS VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.144 RMS AT/cm @Magnetic Field 0.900 T, Frequency 60 Hz | 0.228 RMS VA/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.145 RMS AT/cm @Magnetic Field 0.900 T, Frequency 60 Hz | 0.229 RMS VA/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.163 RMS AT/cm @Magnetic Field 1.10 T, Frequency 50 Hz | 0.258 RMS VA/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.164 RMS AT/cm @Magnetic Field 1.10 T, Frequency 50 Hz | 0.259 RMS VA/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.175 RMS AT/cm @Magnetic Field 1.00 T, Frequency 60 Hz | 0.276 RMS VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.175 RMS AT/cm @Magnetic Field 1.00 T, Frequency 60 Hz | 0.277 RMS VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.196 RMS AT/cm @Magnetic Field 1.20 T, Frequency 50 Hz | 0.309 RMS VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.196 RMS AT/cm @Magnetic Field 1.20 T, Frequency 50 Hz | 0.309 RMS VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.209 RMS AT/cm @Magnetic Field 1.10 T, Frequency 60 Hz | 0.331 RMS VA/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.210 RMS AT/cm @Magnetic Field 1.10 T, Frequency 60 Hz | 0.332 RMS VA/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.235 RMS AT/cm @Magnetic Field 1.30 T, Frequency 50 Hz | 0.371 RMS VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.235 RMS AT/cm @Magnetic Field 1.30 T, Frequency 50 Hz | 0.372 RMS VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.251 RMS AT/cm @Magnetic Field 1.20 T, Frequency 60 Hz | 0.396 RMS VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.251 RMS AT/cm @Magnetic Field 1.20 T, Frequency 60 Hz | 0.396 RMS VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.286 RMS AT/cm @Magnetic Field 1.40 T, Frequency 50 Hz | 0.452 RMS VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.289 RMS AT/cm @Magnetic Field 1.40 T, Frequency 50 Hz | 0.456 RMS VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.300 RMS AT/cm @Magnetic Field 1.30 T, Frequency 60 Hz | 0.474 RMS VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.301 RMS AT/cm @Magnetic Field 1.30 T, Frequency 60 Hz | 0.476 RMS VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.362 RMS AT/cm @Magnetic Field 1.50 T, Frequency 50 Hz | 0.572 RMS VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.364 RMS AT/cm @Magnetic Field 1.40 T, Frequency 60 Hz | 0.575 RMS VA/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.368 RMS AT/cm @Magnetic Field 1.50 T, Frequency 50 Hz | 0.582 RMS VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.457 RMS AT/cm @Magnetic Field 1.50 T, Frequency 60 Hz | 0.722 RMS VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.464 RMS AT/cm @Magnetic Field 1.50 T, Frequency 60 Hz | 0.733 RMS VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.495 RMS AT/cm @Magnetic Field 1.60 T, Frequency 50 Hz | 0.783 RMS VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.499 RMS AT/cm @Magnetic Field 1.60 T, Frequency 50 Hz | 0.788 RMS VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.580 RMS AT/cm @Magnetic Field 1.40 T, Frequency 60 Hz | 0.917 RMS VA/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.617 RMS AT/cm @Magnetic Field 1.60 T, Frequency 60 Hz | 0.975 RMS VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.620 RMS AT/cm @Magnetic Field 1.60 T, Frequency 60 Hz | 0.980 RMS VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.848 RMS AT/cm @Magnetic Field 1.70 T, Frequency 50 Hz | 1.34 RMS VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.917 RMS AT/cm @Magnetic Field 1.70 T, Frequency 50 Hz | 1.45 RMS VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 1.04 RMS AT/cm @Magnetic Field 1.70 T, Frequency 60 Hz | 1.65 RMS VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.13 RMS AT/cm @Magnetic Field 1.70 T, Frequency 60 Hz | 1.78 RMS VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 2.38 RMS AT/cm @Magnetic Field 1.80 T, Frequency 50 Hz | 3.76 RMS VA/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 2.60 RMS AT/cm @Magnetic Field 1.80 T, Frequency 50 Hz | 4.11 RMS VA/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 2.89 RMS AT/cm @Magnetic Field 1.80 T, Frequency 60 Hz | 4.57 RMS VA/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 3.16 RMS AT/cm @Magnetic Field 1.80 T, Frequency 60 Hz | 4.99 RMS VA/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 8.73 RMS AT/cm @Magnetic Field 1.90 T, Frequency 50 Hz | 13.8 RMS VA/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 9.30 RMS AT/cm @Magnetic Field 1.90 T, Frequency 50 Hz | 14.7 RMS VA/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 10.6 RMS AT/cm @Magnetic Field 1.90 T, Frequency 60 Hz | 16.8 RMS VA/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
| 11.4 RMS AT/cm @Magnetic Field 1.90 T, Frequency 60 Hz | 18.0 RMS VA/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
Electrical Resistivity | 0.0000510 ohm-cm | 0.0000510 ohm-cm |
|
Magnetic Properties | Metric | English | Comments |
---|
Core Loss | 0.00430 W/kg @Magnetic Field 0.100 T, Frequency 50 Hz | 0.00195 W/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00430 W/kg @Magnetic Field 0.100 T, Frequency 50 Hz | 0.00195 W/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00571 W/kg @Magnetic Field 0.100 T, Frequency 60 Hz | 0.00259 W/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00573 W/kg @Magnetic Field 0.100 T, Frequency 60 Hz | 0.00260 W/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.0165 W/kg @Magnetic Field 0.200 T, Frequency 50 Hz | 0.00750 W/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0167 W/kg @Magnetic Field 0.200 T, Frequency 50 Hz | 0.00757 W/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0220 W/kg @Magnetic Field 0.200 T, Frequency 60 Hz | 0.0100 W/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0223 W/kg @Magnetic Field 0.200 T, Frequency 60 Hz | 0.0101 W/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0362 W/kg @Magnetic Field 0.300 T, Frequency 50 Hz | 0.0164 W/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0364 W/kg @Magnetic Field 0.300 T, Frequency 50 Hz | 0.0165 W/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0483 W/kg @Magnetic Field 0.300 T, Frequency 60 Hz | 0.0219 W/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0485 W/kg @Magnetic Field 0.300 T, Frequency 60 Hz | 0.0220 W/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0628 W/kg @Magnetic Field 0.400 T, Frequency 50 Hz | 0.0285 W/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0631 W/kg @Magnetic Field 0.400 T, Frequency 50 Hz | 0.0286 W/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0840 W/kg @Magnetic Field 0.400 T, Frequency 60 Hz | 0.0381 W/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0840 W/kg @Magnetic Field 0.400 T, Frequency 60 Hz | 0.0381 W/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0963 W/kg @Magnetic Field 0.500 T, Frequency 50 Hz | 0.0437 W/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0963 W/kg @Magnetic Field 0.500 T, Frequency 50 Hz | 0.0437 W/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.128 W/kg @Magnetic Field 0.500 T, Frequency 60 Hz | 0.0580 W/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.128 W/kg @Magnetic Field 0.500 T, Frequency 60 Hz | 0.0582 W/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.136 W/kg @Magnetic Field 0.600 T, Frequency 50 Hz | 0.0617 W/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.137 W/kg @Magnetic Field 0.600 T, Frequency 50 Hz | 0.0620 W/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.181 W/kg @Magnetic Field 0.600 T, Frequency 60 Hz | 0.0819 W/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.181 W/kg @Magnetic Field 0.600 T, Frequency 60 Hz | 0.0823 W/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.183 W/kg @Magnetic Field 0.700 T, Frequency 50 Hz | 0.0828 W/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.184 W/kg @Magnetic Field 0.700 T, Frequency 50 Hz | 0.0833 W/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.236 W/kg @Magnetic Field 0.800 T, Frequency 50 Hz | 0.107 W/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.238 W/kg @Magnetic Field 0.800 T, Frequency 50 Hz | 0.108 W/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.243 W/kg @Magnetic Field 0.700 T, Frequency 60 Hz | 0.110 W/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.245 W/kg @Magnetic Field 0.700 T, Frequency 60 Hz | 0.111 W/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.295 W/kg @Magnetic Field 0.900 T, Frequency 50 Hz | 0.134 W/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.300 W/kg @Magnetic Field 0.900 T, Frequency 50 Hz | 0.136 W/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.313 W/kg @Magnetic Field 0.800 T, Frequency 60 Hz | 0.142 W/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.315 W/kg @Magnetic Field 0.800 T, Frequency 60 Hz | 0.143 W/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.364 W/kg @Magnetic Field 1.00 T, Frequency 50 Hz | 0.165 W/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.366 W/kg @Magnetic Field 1.00 T, Frequency 50 Hz | 0.166 W/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.392 W/kg @Magnetic Field 0.900 T, Frequency 60 Hz | 0.178 W/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.397 W/kg @Magnetic Field 0.900 T, Frequency 60 Hz | 0.180 W/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.439 W/kg @Magnetic Field 1.10 T, Frequency 50 Hz | 0.199 W/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.443 W/kg @Magnetic Field 1.10 T, Frequency 50 Hz | 0.201 W/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.481 W/kg @Magnetic Field 1.00 T, Frequency 60 Hz | 0.218 W/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.485 W/kg @Magnetic Field 1.00 T, Frequency 60 Hz | 0.220 W/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.525 W/kg @Magnetic Field 1.20 T, Frequency 50 Hz | 0.238 W/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.529 W/kg @Magnetic Field 1.20 T, Frequency 50 Hz | 0.240 W/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.580 W/kg @Magnetic Field 1.10 T, Frequency 60 Hz | 0.263 W/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.586 W/kg @Magnetic Field 1.10 T, Frequency 60 Hz | 0.266 W/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.619 W/kg @Magnetic Field 1.30 T, Frequency 50 Hz | 0.281 W/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.624 W/kg @Magnetic Field 1.30 T, Frequency 50 Hz | 0.283 W/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.692 W/kg @Magnetic Field 1.20 T, Frequency 60 Hz | 0.314 W/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.699 W/kg @Magnetic Field 1.20 T, Frequency 60 Hz | 0.317 W/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.728 W/kg @Magnetic Field 1.40 T, Frequency 50 Hz | 0.330 W/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.732 W/kg @Magnetic Field 1.40 T, Frequency 50 Hz | 0.332 W/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.818 W/kg @Magnetic Field 1.30 T, Frequency 60 Hz | 0.371 W/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.825 W/kg @Magnetic Field 1.30 T, Frequency 60 Hz | 0.374 W/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.860 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz | 0.390 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.860 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz | 0.390 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.860 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz | 0.390 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.959 W/kg @Magnetic Field 1.40 T, Frequency 60 Hz | 0.435 W/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.966 W/kg @Magnetic Field 1.40 T, Frequency 60 Hz | 0.438 W/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| <= 0.970 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz | <= 0.440 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 1.02 W/kg @Magnetic Field 1.60 T, Frequency 50 Hz | 0.462 W/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 1.02 W/kg @Magnetic Field 1.60 T, Frequency 50 Hz | 0.463 W/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 1.13 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz | 0.513 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 1.13 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz | 0.513 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 1.13 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz | 0.513 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 1.24 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | 0.563 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 1.25 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | 0.566 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 1.25 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | 0.566 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| <= 1.28 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz | <= 0.580 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 1.33 W/kg @Magnetic Field 1.60 T, Frequency 60 Hz | 0.605 W/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 1.34 W/kg @Magnetic Field 1.60 T, Frequency 60 Hz | 0.606 W/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| <= 1.39 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | <= 0.630 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 1.58 W/kg @Magnetic Field 1.80 T, Frequency 50 Hz | 0.717 W/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 1.59 W/kg @Magnetic Field 1.80 T, Frequency 50 Hz | 0.719 W/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 1.62 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | 0.733 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.62 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | 0.735 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.62 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | 0.736 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| <= 1.83 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | <= 0.830 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.97 W/kg @Magnetic Field 1.90 T, Frequency 50 Hz | 0.895 W/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 1.98 W/kg @Magnetic Field 1.90 T, Frequency 50 Hz | 0.898 W/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 2.04 W/kg @Magnetic Field 1.80 T, Frequency 60 Hz | 0.925 W/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 2.05 W/kg @Magnetic Field 1.80 T, Frequency 60 Hz | 0.930 W/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 2.54 W/kg @Magnetic Field 1.90 T, Frequency 60 Hz | 1.15 W/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
| 2.54 W/kg @Magnetic Field 1.90 T, Frequency 60 Hz | 1.15 W/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
|
Descriptive Properties |
---|
Magnetostriction 10^8 | -125 |
| -94 |
Minimum Lamination Factor (%) | 95.5 |
Minimum Peak Permeability at 10 Oe | 1780 |
Typical Lamination Factor (%) | 97.2 |
Typical Peak Permeability at 10 Oe | 1834 |