Physical Properties | Metric | English | Comments |
---|
Density | 7.65 g/cc | 0.276 lb/in³ |
Thickness | 356 microns | 14.0 mil |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Knoop | 167 | 167 |
Hardness, Rockwell B | 81 | 81 |
Tensile Strength, Ultimate | 352 MPa | 51000 psi |
Tensile Strength, Yield | 331 MPa | 48000 psi |
Elongation at Break | 9.0 % | 9.0 % |
Modulus of Elasticity | 122 GPa | 17700 ksi |
| 143 GPa | 20700 ksi |
| 200 GPa | 29000 ksi |
| 236 GPa | 34200 ksi |
| 258 GPa | 37400 ksi |
|
Electrical Properties | Metric | English | Comments |
---|
Exciting Power (RMS) | 0.00249 RMS AT/cm @Magnetic Field 0.100 T, Frequency 50 Hz | 0.00393 RMS VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00257 RMS AT/cm @Magnetic Field 0.100 T, Frequency 50 Hz | 0.00406 RMS VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00316 RMS AT/cm @Magnetic Field 0.100 T, Frequency 60 Hz | 0.00499 RMS VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00326 RMS AT/cm @Magnetic Field 0.100 T, Frequency 60 Hz | 0.00516 RMS VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00835 RMS AT/cm @Magnetic Field 0.200 T, Frequency 50 Hz | 0.0132 RMS VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.00848 RMS AT/cm @Magnetic Field 0.200 T, Frequency 50 Hz | 0.0134 RMS VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0107 RMS AT/cm @Magnetic Field 0.200 T, Frequency 60 Hz | 0.0169 RMS VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0109 RMS AT/cm @Magnetic Field 0.200 T, Frequency 60 Hz | 0.0173 RMS VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0169 RMS AT/cm @Magnetic Field 0.300 T, Frequency 50 Hz | 0.0267 RMS VA/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0171 RMS AT/cm @Magnetic Field 0.300 T, Frequency 50 Hz | 0.0270 RMS VA/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0219 RMS AT/cm @Magnetic Field 0.300 T, Frequency 60 Hz | 0.0346 RMS VA/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0221 RMS AT/cm @Magnetic Field 0.300 T, Frequency 60 Hz | 0.0350 RMS VA/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0278 RMS AT/cm @Magnetic Field 0.400 T, Frequency 50 Hz | 0.0440 RMS VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0280 RMS AT/cm @Magnetic Field 0.400 T, Frequency 50 Hz | 0.0443 RMS VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0362 RMS AT/cm @Magnetic Field 0.400 T, Frequency 60 Hz | 0.0572 RMS VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0364 RMS AT/cm @Magnetic Field 0.400 T, Frequency 60 Hz | 0.0576 RMS VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0410 RMS AT/cm @Magnetic Field 0.500 T, Frequency 50 Hz | 0.0648 RMS VA/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0412 RMS AT/cm @Magnetic Field 0.500 T, Frequency 50 Hz | 0.0651 RMS VA/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0534 RMS AT/cm @Magnetic Field 0.500 T, Frequency 60 Hz | 0.0844 RMS VA/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0537 RMS AT/cm @Magnetic Field 0.500 T, Frequency 60 Hz | 0.0848 RMS VA/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0562 RMS AT/cm @Magnetic Field 0.600 T, Frequency 50 Hz | 0.0889 RMS VA/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0565 RMS AT/cm @Magnetic Field 0.600 T, Frequency 50 Hz | 0.0893 RMS VA/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0734 RMS AT/cm @Magnetic Field 0.600 T, Frequency 60 Hz | 0.116 RMS VA/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.0734 RMS AT/cm @Magnetic Field 0.700 T, Frequency 50 Hz | 0.116 RMS VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.0734 RMS AT/cm @Magnetic Field 0.600 T, Frequency 60 Hz | 0.116 RMS VA/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.0740 RMS AT/cm @Magnetic Field 0.700 T, Frequency 50 Hz | 0.117 RMS VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.0930 RMS AT/cm @Magnetic Field 0.800 T, Frequency 50 Hz | 0.147 RMS VA/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.0936 RMS AT/cm @Magnetic Field 0.800 T, Frequency 50 Hz | 0.148 RMS VA/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.0962 RMS AT/cm @Magnetic Field 0.700 T, Frequency 60 Hz | 0.152 RMS VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.0968 RMS AT/cm @Magnetic Field 0.700 T, Frequency 60 Hz | 0.153 RMS VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.115 RMS AT/cm @Magnetic Field 0.900 T, Frequency 50 Hz | 0.182 RMS VA/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.116 RMS AT/cm @Magnetic Field 0.900 T, Frequency 50 Hz | 0.183 RMS VA/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.122 RMS AT/cm @Magnetic Field 0.800 T, Frequency 60 Hz | 0.193 RMS VA/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.122 RMS AT/cm @Magnetic Field 0.800 T, Frequency 60 Hz | 0.193 RMS VA/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.140 RMS AT/cm @Magnetic Field 1.00 T, Frequency 50 Hz | 0.221 RMS VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.140 RMS AT/cm @Magnetic Field 1.00 T, Frequency 50 Hz | 0.222 RMS VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.151 RMS AT/cm @Magnetic Field 0.900 T, Frequency 60 Hz | 0.238 RMS VA/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.151 RMS AT/cm @Magnetic Field 0.900 T, Frequency 60 Hz | 0.239 RMS VA/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.167 RMS AT/cm @Magnetic Field 1.10 T, Frequency 50 Hz | 0.264 RMS VA/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.168 RMS AT/cm @Magnetic Field 1.10 T, Frequency 50 Hz | 0.266 RMS VA/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.182 RMS AT/cm @Magnetic Field 1.00 T, Frequency 60 Hz | 0.288 RMS VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.183 RMS AT/cm @Magnetic Field 1.00 T, Frequency 60 Hz | 0.290 RMS VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.199 RMS AT/cm @Magnetic Field 1.20 T, Frequency 50 Hz | 0.314 RMS VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.201 RMS AT/cm @Magnetic Field 1.20 T, Frequency 50 Hz | 0.318 RMS VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.218 RMS AT/cm @Magnetic Field 1.10 T, Frequency 60 Hz | 0.345 RMS VA/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.220 RMS AT/cm @Magnetic Field 1.10 T, Frequency 60 Hz | 0.348 RMS VA/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.235 RMS AT/cm @Magnetic Field 1.30 T, Frequency 50 Hz | 0.372 RMS VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.240 RMS AT/cm @Magnetic Field 1.30 T, Frequency 50 Hz | 0.379 RMS VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.259 RMS AT/cm @Magnetic Field 1.20 T, Frequency 60 Hz | 0.409 RMS VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.262 RMS AT/cm @Magnetic Field 1.20 T, Frequency 60 Hz | 0.414 RMS VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.281 RMS AT/cm @Magnetic Field 1.40 T, Frequency 50 Hz | 0.444 RMS VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.289 RMS AT/cm @Magnetic Field 1.40 T, Frequency 50 Hz | 0.456 RMS VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.306 RMS AT/cm @Magnetic Field 1.30 T, Frequency 60 Hz | 0.484 RMS VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.312 RMS AT/cm @Magnetic Field 1.30 T, Frequency 60 Hz | 0.493 RMS VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.344 RMS AT/cm @Magnetic Field 1.50 T, Frequency 50 Hz | 0.544 RMS VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.361 RMS AT/cm @Magnetic Field 1.50 T, Frequency 50 Hz | 0.571 RMS VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.364 RMS AT/cm @Magnetic Field 1.40 T, Frequency 60 Hz | 0.575 RMS VA/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.442 RMS AT/cm @Magnetic Field 1.50 T, Frequency 60 Hz | 0.699 RMS VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.451 RMS AT/cm @Magnetic Field 1.60 T, Frequency 50 Hz | 0.713 RMS VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.464 RMS AT/cm @Magnetic Field 1.50 T, Frequency 60 Hz | 0.734 RMS VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.481 RMS AT/cm @Magnetic Field 1.60 T, Frequency 50 Hz | 0.761 RMS VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.572 RMS AT/cm @Magnetic Field 1.60 T, Frequency 60 Hz | 0.904 RMS VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.591 RMS AT/cm @Magnetic Field 1.40 T, Frequency 60 Hz | 0.934 RMS VA/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.611 RMS AT/cm @Magnetic Field 1.60 T, Frequency 60 Hz | 0.965 RMS VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.734 RMS AT/cm @Magnetic Field 1.70 T, Frequency 50 Hz | 1.16 RMS VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.873 RMS AT/cm @Magnetic Field 1.70 T, Frequency 50 Hz | 1.38 RMS VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.905 RMS AT/cm @Magnetic Field 1.70 T, Frequency 60 Hz | 1.43 RMS VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.08 RMS AT/cm @Magnetic Field 1.70 T, Frequency 60 Hz | 1.71 RMS VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 2.17 RMS AT/cm @Magnetic Field 1.80 T, Frequency 50 Hz | 3.43 RMS VA/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 2.61 RMS AT/cm @Magnetic Field 1.80 T, Frequency 60 Hz | 4.13 RMS VA/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 2.63 RMS AT/cm @Magnetic Field 1.80 T, Frequency 50 Hz | 4.16 RMS VA/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 3.17 RMS AT/cm @Magnetic Field 1.80 T, Frequency 60 Hz | 5.01 RMS VA/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 9.11 RMS AT/cm @Magnetic Field 1.90 T, Frequency 50 Hz | 14.4 RMS VA/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 9.62 RMS AT/cm @Magnetic Field 1.90 T, Frequency 50 Hz | 15.2 RMS VA/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 10.9 RMS AT/cm @Magnetic Field 1.90 T, Frequency 60 Hz | 17.2 RMS VA/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
| 11.5 RMS AT/cm @Magnetic Field 1.90 T, Frequency 60 Hz | 18.2 RMS VA/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
Electrical Resistivity | 0.0000510 ohm-cm | 0.0000510 ohm-cm |
|
Magnetic Properties | Metric | English | Comments |
---|
Core Loss | 0.00545 W/kg @Magnetic Field 0.100 T, Frequency 50 Hz | 0.00247 W/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00553 W/kg @Magnetic Field 0.100 T, Frequency 50 Hz | 0.00251 W/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00725 W/kg @Magnetic Field 0.100 T, Frequency 60 Hz | 0.00329 W/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00736 W/kg @Magnetic Field 0.100 T, Frequency 60 Hz | 0.00334 W/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.0203 W/kg @Magnetic Field 0.200 T, Frequency 50 Hz | 0.00921 W/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0205 W/kg @Magnetic Field 0.200 T, Frequency 50 Hz | 0.00928 W/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0271 W/kg @Magnetic Field 0.200 T, Frequency 60 Hz | 0.0123 W/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0273 W/kg @Magnetic Field 0.200 T, Frequency 60 Hz | 0.0124 W/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0434 W/kg @Magnetic Field 0.300 T, Frequency 50 Hz | 0.0197 W/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0439 W/kg @Magnetic Field 0.300 T, Frequency 50 Hz | 0.0199 W/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0584 W/kg @Magnetic Field 0.300 T, Frequency 60 Hz | 0.0265 W/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0589 W/kg @Magnetic Field 0.300 T, Frequency 60 Hz | 0.0267 W/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0745 W/kg @Magnetic Field 0.400 T, Frequency 50 Hz | 0.0338 W/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0754 W/kg @Magnetic Field 0.400 T, Frequency 50 Hz | 0.0342 W/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0999 W/kg @Magnetic Field 0.400 T, Frequency 60 Hz | 0.0453 W/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.101 W/kg @Magnetic Field 0.400 T, Frequency 60 Hz | 0.0458 W/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.113 W/kg @Magnetic Field 0.500 T, Frequency 50 Hz | 0.0513 W/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.114 W/kg @Magnetic Field 0.500 T, Frequency 50 Hz | 0.0518 W/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.151 W/kg @Magnetic Field 0.500 T, Frequency 60 Hz | 0.0687 W/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.153 W/kg @Magnetic Field 0.500 T, Frequency 60 Hz | 0.0694 W/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.159 W/kg @Magnetic Field 0.600 T, Frequency 50 Hz | 0.0721 W/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.160 W/kg @Magnetic Field 0.600 T, Frequency 50 Hz | 0.0728 W/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.213 W/kg @Magnetic Field 0.700 T, Frequency 50 Hz | 0.0964 W/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.213 W/kg @Magnetic Field 0.600 T, Frequency 60 Hz | 0.0964 W/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.214 W/kg @Magnetic Field 0.700 T, Frequency 50 Hz | 0.0971 W/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.215 W/kg @Magnetic Field 0.600 T, Frequency 60 Hz | 0.0973 W/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.273 W/kg @Magnetic Field 0.800 T, Frequency 50 Hz | 0.124 W/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.276 W/kg @Magnetic Field 0.800 T, Frequency 50 Hz | 0.125 W/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.284 W/kg @Magnetic Field 0.700 T, Frequency 60 Hz | 0.129 W/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.287 W/kg @Magnetic Field 0.700 T, Frequency 60 Hz | 0.130 W/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.342 W/kg @Magnetic Field 0.900 T, Frequency 50 Hz | 0.155 W/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.344 W/kg @Magnetic Field 0.900 T, Frequency 50 Hz | 0.156 W/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.364 W/kg @Magnetic Field 0.800 T, Frequency 60 Hz | 0.165 W/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.366 W/kg @Magnetic Field 0.800 T, Frequency 60 Hz | 0.166 W/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.419 W/kg @Magnetic Field 1.00 T, Frequency 50 Hz | 0.190 W/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.421 W/kg @Magnetic Field 1.00 T, Frequency 50 Hz | 0.191 W/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.456 W/kg @Magnetic Field 0.900 T, Frequency 60 Hz | 0.207 W/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.459 W/kg @Magnetic Field 0.900 T, Frequency 60 Hz | 0.208 W/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.505 W/kg @Magnetic Field 1.10 T, Frequency 50 Hz | 0.229 W/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.507 W/kg @Magnetic Field 1.10 T, Frequency 50 Hz | 0.230 W/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.558 W/kg @Magnetic Field 1.00 T, Frequency 60 Hz | 0.253 W/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.560 W/kg @Magnetic Field 1.00 T, Frequency 60 Hz | 0.254 W/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.602 W/kg @Magnetic Field 1.20 T, Frequency 50 Hz | 0.273 W/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.602 W/kg @Magnetic Field 1.20 T, Frequency 50 Hz | 0.273 W/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.672 W/kg @Magnetic Field 1.10 T, Frequency 60 Hz | 0.305 W/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.672 W/kg @Magnetic Field 1.10 T, Frequency 60 Hz | 0.305 W/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.708 W/kg @Magnetic Field 1.30 T, Frequency 50 Hz | 0.321 W/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.710 W/kg @Magnetic Field 1.30 T, Frequency 50 Hz | 0.322 W/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.798 W/kg @Magnetic Field 1.20 T, Frequency 60 Hz | 0.362 W/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.800 W/kg @Magnetic Field 1.20 T, Frequency 60 Hz | 0.363 W/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.827 W/kg @Magnetic Field 1.40 T, Frequency 50 Hz | 0.375 W/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.829 W/kg @Magnetic Field 1.40 T, Frequency 50 Hz | 0.376 W/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.937 W/kg @Magnetic Field 1.30 T, Frequency 60 Hz | 0.425 W/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.941 W/kg @Magnetic Field 1.30 T, Frequency 60 Hz | 0.427 W/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.963 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz | 0.437 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.970 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz | 0.440 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.970 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz | 0.440 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 1.09 W/kg @Magnetic Field 1.40 T, Frequency 60 Hz | 0.496 W/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 1.10 W/kg @Magnetic Field 1.40 T, Frequency 60 Hz | 0.498 W/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| <= 1.10 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz | <= 0.500 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 1.13 W/kg @Magnetic Field 1.60 T, Frequency 50 Hz | 0.512 W/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 1.14 W/kg @Magnetic Field 1.60 T, Frequency 50 Hz | 0.517 W/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 1.27 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz | 0.578 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 1.28 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz | 0.582 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 1.28 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz | 0.582 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 1.35 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | 0.612 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 1.38 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | 0.625 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 1.38 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | 0.627 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| <= 1.46 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz | <= 0.660 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 1.49 W/kg @Magnetic Field 1.60 T, Frequency 60 Hz | 0.676 W/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 1.51 W/kg @Magnetic Field 1.60 T, Frequency 60 Hz | 0.683 W/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| <= 1.57 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | <= 0.710 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 1.69 W/kg @Magnetic Field 1.80 T, Frequency 50 Hz | 0.765 W/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 1.71 W/kg @Magnetic Field 1.80 T, Frequency 50 Hz | 0.776 W/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 1.78 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | 0.806 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.81 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | 0.823 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.81 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | 0.823 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 2.03 W/kg @Magnetic Field 1.90 T, Frequency 50 Hz | 0.921 W/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| <= 2.07 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | <= 0.940 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 2.08 W/kg @Magnetic Field 1.90 T, Frequency 50 Hz | 0.943 W/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 2.20 W/kg @Magnetic Field 1.80 T, Frequency 60 Hz | 1.00 W/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 2.25 W/kg @Magnetic Field 1.80 T, Frequency 60 Hz | 1.02 W/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 2.62 W/kg @Magnetic Field 1.90 T, Frequency 60 Hz | 1.19 W/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
| 2.69 W/kg @Magnetic Field 1.90 T, Frequency 60 Hz | 1.22 W/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
|
Descriptive Properties |
---|
Magnetostriction 10^8 | -124 |
| -97 |
Minimum Lamination Factor (%) | 96 |
Minimum Peak Permeability at 10 Oe | 1780 |
Typical Lamination Factor (%) | 97.2 |
Typical Peak Permeability at 10 Oe | 1848 |