Physical Properties | Original Value | Comments |
---|
Density | 7.65 g/cc |
Thickness | 14.0 mil |
|
Mechanical Properties | Original Value | Comments |
---|
Hardness, Knoop | 167 |
Hardness, Rockwell B | 81 |
Tensile Strength, Ultimate | 51000 psi |
Tensile Strength, Yield | 48000 psi |
Elongation at Break | 9.0 % |
Modulus of Elasticity | 122 GPa |
| 143 GPa |
| 200 GPa |
| 236 GPa |
| 258 GPa |
|
Electrical Properties | Original Value | Comments |
---|
Exciting Power (RMS) | 0.00393 RMS VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00406 RMS VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00499 RMS VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00516 RMS VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.0132 RMS VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0134 RMS VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0169 RMS VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0173 RMS VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0267 RMS VA/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0270 RMS VA/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0346 RMS VA/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0350 RMS VA/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0440 RMS VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0443 RMS VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0572 RMS VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0576 RMS VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0648 RMS VA/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0651 RMS VA/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0844 RMS VA/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0848 RMS VA/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0889 RMS VA/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0893 RMS VA/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.116 RMS VA/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.116 RMS VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.116 RMS VA/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.117 RMS VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.147 RMS VA/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.148 RMS VA/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.152 RMS VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.153 RMS VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.182 RMS VA/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.183 RMS VA/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.193 RMS VA/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.193 RMS VA/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.221 RMS VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.222 RMS VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.238 RMS VA/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.239 RMS VA/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.264 RMS VA/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.266 RMS VA/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.288 RMS VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.290 RMS VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.314 RMS VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.318 RMS VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.345 RMS VA/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.348 RMS VA/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.372 RMS VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.379 RMS VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.409 RMS VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.414 RMS VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.444 RMS VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.456 RMS VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.484 RMS VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.493 RMS VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.544 RMS VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.571 RMS VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.575 RMS VA/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.591 RMS AT/cm @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.699 RMS VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.713 RMS VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.734 RMS VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.761 RMS VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.904 RMS VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.965 RMS VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 1.16 RMS VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 1.38 RMS VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 1.43 RMS VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.71 RMS VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 3.43 RMS VA/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 4.13 RMS VA/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 4.16 RMS VA/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 5.01 RMS VA/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 14.4 RMS VA/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 15.2 RMS VA/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 17.2 RMS VA/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
| 18.2 RMS VA/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
Electrical Resistivity | 0.0000510 ohm-cm |
|
Magnetic Properties | Original Value | Comments |
---|
Core Loss | 0.00247 W/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00251 W/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00329 W/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00334 W/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00921 W/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.00928 W/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0123 W/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0124 W/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0197 W/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0199 W/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0265 W/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0267 W/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0338 W/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0342 W/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0453 W/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0458 W/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0513 W/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0518 W/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0687 W/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0694 W/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0721 W/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0728 W/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0964 W/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.0964 W/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.0971 W/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.0973 W/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.124 W/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.125 W/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.129 W/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.130 W/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.155 W/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.156 W/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.165 W/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.166 W/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.190 W/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.191 W/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.207 W/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.208 W/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.229 W/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.230 W/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.253 W/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.254 W/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.273 W/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.273 W/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.305 W/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.305 W/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.321 W/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.322 W/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.362 W/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.363 W/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.375 W/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.376 W/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.425 W/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.427 W/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.437 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.440 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.440 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.496 W/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.498 W/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| <= 0.500 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.512 W/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.517 W/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.578 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.582 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.582 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.612 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.625 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.627 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| <= 0.660 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.676 W/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.683 W/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| <= 0.710 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.765 W/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 0.776 W/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 0.806 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 0.823 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 0.823 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 0.921 W/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| <= 0.940 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 0.943 W/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 1.00 W/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 1.02 W/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 1.19 W/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
| 1.22 W/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
|
Descriptive Properties |
---|
Magnetostriction 10^8 | -124 |
| -97 |
Minimum Lamination Factor (%) | 96 |
Minimum Peak Permeability at 10 Oe | 1780 |
Typical Lamination Factor (%) | 97.2 |
Typical Peak Permeability at 10 Oe | 1848 |