MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AK Steel DI-MAX® HF-10 Nonoriented Electrical Steel (Extended Electrical/Magnetic Data)
Categories: Metal; Electronic/Magnetic Alloy; Ferrous Metal

Material Notes: DI-MAX HF-10 is a fully processed nonoriented electrical steel designed for use in high speed motors, traction motors, aircraft generators, and other rotating equipment operating at frequencies above 60 Hz. DI-MAX HF-10 Electrical Steel is supplied in a nominal thickness of 0.25 mm (0.010 in).

Information provided by AK Steel.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.65 g/cc0.276 lb/in³ASTM A34
Thickness 250 microns9.84 milAim
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 7878
Tensile Strength, Ultimate 450 MPa65300 psi
Tensile Strength, Yield 350 MPa50800 psi
Elongation at Break 20 %20 %In 2"
 
Electrical PropertiesMetricEnglishComments
Exciting Power  0.0188 VA/lb
@Magnetic Field 0.100 T,
Frequency 50 Hz
0.0188 VA/lb
@Magnetic Field 0.100 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.0226 VA/lb
@Magnetic Field 0.100 T,
Frequency 60 Hz
0.0226 VA/lb
@Magnetic Field 0.100 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.0226 VA/lb
@Magnetic Field 0.100 T,
Frequency 50 Hz
0.0226 VA/lb
@Magnetic Field 0.100 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.0273 VA/lb
@Magnetic Field 0.100 T,
Frequency 60 Hz
0.0273 VA/lb
@Magnetic Field 0.100 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.0385 VA/lb
@Magnetic Field 0.100 T,
Frequency 100 Hz
0.0385 VA/lb
@Magnetic Field 0.100 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.0459 VA/lb
@Magnetic Field 0.100 T,
Frequency 100 Hz
0.0459 VA/lb
@Magnetic Field 0.100 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.0536 VA/lb
@Magnetic Field 0.200 T,
Frequency 50 Hz
0.0536 VA/lb
@Magnetic Field 0.200 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.0650 VA/lb
@Magnetic Field 0.200 T,
Frequency 60 Hz
0.0650 VA/lb
@Magnetic Field 0.200 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.0650 VA/lb
@Magnetic Field 0.200 T,
Frequency 50 Hz
0.0650 VA/lb
@Magnetic Field 0.200 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.0786 VA/lb
@Magnetic Field 0.200 T,
Frequency 60 Hz
0.0786 VA/lb
@Magnetic Field 0.200 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.0800 VA/lb
@Magnetic Field 0.100 T,
Frequency 200 Hz
0.0800 VA/lb
@Magnetic Field 0.100 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.0941 VA/lb
@Magnetic Field 0.100 T,
Frequency 200 Hz
0.0941 VA/lb
@Magnetic Field 0.100 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.1118 VA/lb
@Magnetic Field 0.200 T,
Frequency 100 Hz
0.1118 VA/lb
@Magnetic Field 0.200 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.1336 VA/lb
@Magnetic Field 0.200 T,
Frequency 100 Hz
0.1336 VA/lb
@Magnetic Field 0.200 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.1464 VA/lb
@Magnetic Field 0.400 T,
Frequency 50 Hz
0.1464 VA/lb
@Magnetic Field 0.400 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.1714 VA/lb
@Magnetic Field 0.100 T,
Frequency 400 Hz
0.1714 VA/lb
@Magnetic Field 0.100 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.1768 VA/lb
@Magnetic Field 0.400 T,
Frequency 50 Hz
0.1768 VA/lb
@Magnetic Field 0.400 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.1773 VA/lb
@Magnetic Field 0.400 T,
Frequency 60 Hz
0.1773 VA/lb
@Magnetic Field 0.400 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.1968 VA/lb
@Magnetic Field 0.100 T,
Frequency 400 Hz
0.1968 VA/lb
@Magnetic Field 0.100 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.2141 VA/lb
@Magnetic Field 0.400 T,
Frequency 60 Hz
0.2141 VA/lb
@Magnetic Field 0.400 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.2373 VA/lb
@Magnetic Field 0.200 T,
Frequency 200 Hz
0.2373 VA/lb
@Magnetic Field 0.200 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.2805 VA/lb
@Magnetic Field 0.200 T,
Frequency 200 Hz
0.2805 VA/lb
@Magnetic Field 0.200 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.310 VA/lb
@Magnetic Field 0.400 T,
Frequency 100 Hz
0.310 VA/lb
@Magnetic Field 0.400 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.3273 VA/lb
@Magnetic Field 0.100 T,
Frequency 700 Hz
0.3273 VA/lb
@Magnetic Field 0.100 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.3386 VA/lb
@Magnetic Field 0.700 T,
Frequency 50 Hz
0.3386 VA/lb
@Magnetic Field 0.700 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.3677 VA/lb
@Magnetic Field 0.100 T,
Frequency 700 Hz
0.3677 VA/lb
@Magnetic Field 0.100 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.3686 VA/lb
@Magnetic Field 0.400 T,
Frequency 100 Hz
0.3686 VA/lb
@Magnetic Field 0.400 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.4114 VA/lb
@Magnetic Field 0.700 T,
Frequency 50 Hz
0.4114 VA/lb
@Magnetic Field 0.700 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.4123 VA/lb
@Magnetic Field 0.700 T,
Frequency 60 Hz
0.4123 VA/lb
@Magnetic Field 0.700 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.4455 VA/lb
@Magnetic Field 0.100 T,
Frequency 1000 Hz
0.4455 VA/lb
@Magnetic Field 0.100 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.500 VA/lb
@Magnetic Field 0.700 T,
Frequency 60 Hz
0.500 VA/lb
@Magnetic Field 0.700 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.5318 VA/lb
@Magnetic Field 0.200 T,
Frequency 400 Hz
0.5318 VA/lb
@Magnetic Field 0.200 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.5636 VA/lb
@Magnetic Field 0.100 T,
Frequency 1000 Hz
0.5636 VA/lb
@Magnetic Field 0.100 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.6091 VA/lb
@Magnetic Field 0.200 T,
Frequency 400 Hz
0.6091 VA/lb
@Magnetic Field 0.200 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.650 VA/lb
@Magnetic Field 1.00 T,
Frequency 50 Hz
0.650 VA/lb
@Magnetic Field 1.00 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.6818 VA/lb
@Magnetic Field 0.400 T,
Frequency 200 Hz
0.6818 VA/lb
@Magnetic Field 0.400 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.7273 VA/lb
@Magnetic Field 0.700 T,
Frequency 100 Hz
0.7273 VA/lb
@Magnetic Field 0.700 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.7909 VA/lb
@Magnetic Field 1.00 T,
Frequency 60 Hz
0.7909 VA/lb
@Magnetic Field 1.00 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.7955 VA/lb
@Magnetic Field 0.400 T,
Frequency 200 Hz
0.7955 VA/lb
@Magnetic Field 0.400 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.800 VA/lb
@Magnetic Field 1.00 T,
Frequency 50 Hz
0.800 VA/lb
@Magnetic Field 1.00 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.8636 VA/lb
@Magnetic Field 0.700 T,
Frequency 100 Hz
0.8636 VA/lb
@Magnetic Field 0.700 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.900 VA/lb
@Magnetic Field 0.100 T,
Frequency 1500 Hz
0.900 VA/lb
@Magnetic Field 0.100 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.9364 VA/lb
@Magnetic Field 0.100 T,
Frequency 1500 Hz
0.9364 VA/lb
@Magnetic Field 0.100 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.9682 VA/lb
@Magnetic Field 1.00 T,
Frequency 60 Hz
0.9682 VA/lb
@Magnetic Field 1.00 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 1.0636 VA/lb
@Magnetic Field 0.200 T,
Frequency 700 Hz
1.0636 VA/lb
@Magnetic Field 0.200 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 1.0773 VA/lb
@Magnetic Field 1.20 T,
Frequency 50 Hz
1.0773 VA/lb
@Magnetic Field 1.20 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 1.1909 VA/lb
@Magnetic Field 0.200 T,
Frequency 700 Hz
1.1909 VA/lb
@Magnetic Field 0.200 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 1.3045 VA/lb
@Magnetic Field 1.20 T,
Frequency 60 Hz
1.3045 VA/lb
@Magnetic Field 1.20 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 1.3364 VA/lb
@Magnetic Field 1.20 T,
Frequency 50 Hz
1.3364 VA/lb
@Magnetic Field 1.20 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 1.3864 VA/lb
@Magnetic Field 1.00 T,
Frequency 100 Hz
1.3864 VA/lb
@Magnetic Field 1.00 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 1.5591 VA/lb
@Magnetic Field 0.200 T,
Frequency 1000 Hz
1.5591 VA/lb
@Magnetic Field 0.200 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 1.5864 VA/lb
@Magnetic Field 0.400 T,
Frequency 400 Hz
1.5864 VA/lb
@Magnetic Field 0.400 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 1.5864 VA/lb
@Magnetic Field 1.30 T,
Frequency 50 Hz
1.5864 VA/lb
@Magnetic Field 1.30 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 1.6136 VA/lb
@Magnetic Field 1.20 T,
Frequency 60 Hz
1.6136 VA/lb
@Magnetic Field 1.20 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 1.6318 VA/lb
@Magnetic Field 0.700 T,
Frequency 200 Hz
1.6318 VA/lb
@Magnetic Field 0.700 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 1.6682 VA/lb
@Magnetic Field 1.00 T,
Frequency 100 Hz
1.6682 VA/lb
@Magnetic Field 1.00 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 1.8045 VA/lb
@Magnetic Field 0.400 T,
Frequency 400 Hz
1.8045 VA/lb
@Magnetic Field 0.400 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 1.8591 VA/lb
@Magnetic Field 0.100 T,
Frequency 2500 Hz
1.8591 VA/lb
@Magnetic Field 0.100 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 1.8818 VA/lb
@Magnetic Field 0.200 T,
Frequency 1000 Hz
1.8818 VA/lb
@Magnetic Field 0.200 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 1.8909 VA/lb
@Magnetic Field 0.700 T,
Frequency 200 Hz
1.8909 VA/lb
@Magnetic Field 0.700 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 1.8955 VA/lb
@Magnetic Field 0.100 T,
Frequency 2500 Hz
1.8955 VA/lb
@Magnetic Field 0.100 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 1.9273 VA/lb
@Magnetic Field 1.30 T,
Frequency 60 Hz
1.9273 VA/lb
@Magnetic Field 1.30 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 1.9591 VA/lb
@Magnetic Field 1.30 T,
Frequency 50 Hz
1.9591 VA/lb
@Magnetic Field 1.30 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 2.25 VA/lb
@Magnetic Field 1.20 T,
Frequency 100 Hz
2.25 VA/lb
@Magnetic Field 1.20 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 2.3636 VA/lb
@Magnetic Field 1.30 T,
Frequency 60 Hz
2.3636 VA/lb
@Magnetic Field 1.30 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 2.7545 VA/lb
@Magnetic Field 1.20 T,
Frequency 100 Hz
2.7545 VA/lb
@Magnetic Field 1.20 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 3.0727 VA/lb
@Magnetic Field 0.200 T,
Frequency 1500 Hz
3.0727 VA/lb
@Magnetic Field 0.200 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 3.10 VA/lb
@Magnetic Field 1.00 T,
Frequency 200 Hz
3.10 VA/lb
@Magnetic Field 1.00 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 3.2364 VA/lb
@Magnetic Field 0.200 T,
Frequency 1500 Hz
3.2364 VA/lb
@Magnetic Field 0.200 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 3.2864 VA/lb
@Magnetic Field 1.30 T,
Frequency 100 Hz
3.2864 VA/lb
@Magnetic Field 1.30 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 3.3409 VA/lb
@Magnetic Field 0.400 T,
Frequency 700 Hz
3.3409 VA/lb
@Magnetic Field 0.400 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 3.3455 VA/lb
@Magnetic Field 1.40 T,
Frequency 50 Hz
3.3455 VA/lb
@Magnetic Field 1.40 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 3.6273 VA/lb
@Magnetic Field 1.00 T,
Frequency 200 Hz
3.6273 VA/lb
@Magnetic Field 1.00 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 3.6682 VA/lb
@Magnetic Field 0.400 T,
Frequency 700 Hz
3.6682 VA/lb
@Magnetic Field 0.400 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 3.7818 VA/lb
@Magnetic Field 1.40 T,
Frequency 50 Hz
3.7818 VA/lb
@Magnetic Field 1.40 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 3.9318 VA/lb
@Magnetic Field 0.700 T,
Frequency 400 Hz
3.9318 VA/lb
@Magnetic Field 0.700 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 3.9955 VA/lb
@Magnetic Field 1.30 T,
Frequency 100 Hz
3.9955 VA/lb
@Magnetic Field 1.30 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 4.0636 VA/lb
@Magnetic Field 1.40 T,
Frequency 60 Hz
4.0636 VA/lb
@Magnetic Field 1.40 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 4.4182 VA/lb
@Magnetic Field 0.700 T,
Frequency 400 Hz
4.4182 VA/lb
@Magnetic Field 0.700 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 4.5455 VA/lb
@Magnetic Field 1.40 T,
Frequency 60 Hz
4.5455 VA/lb
@Magnetic Field 1.40 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 4.9091 VA/lb
@Magnetic Field 1.20 T,
Frequency 200 Hz
4.9091 VA/lb
@Magnetic Field 1.20 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 5.2273 VA/lb
@Magnetic Field 0.400 T,
Frequency 1000 Hz
5.2273 VA/lb
@Magnetic Field 0.400 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 5.5455 VA/lb
@Magnetic Field 0.100 T,
Frequency 5000 Hz
5.5455 VA/lb
@Magnetic Field 0.100 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 5.6818 VA/lb
@Magnetic Field 0.100 T,
Frequency 5000 Hz
5.6818 VA/lb
@Magnetic Field 0.100 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 5.8636 VA/lb
@Magnetic Field 1.20 T,
Frequency 200 Hz
5.8636 VA/lb
@Magnetic Field 1.20 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 5.9545 VA/lb
@Magnetic Field 0.400 T,
Frequency 1000 Hz
5.9545 VA/lb
@Magnetic Field 0.400 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 6.5909 VA/lb
@Magnetic Field 0.200 T,
Frequency 2500 Hz
6.5909 VA/lb
@Magnetic Field 0.200 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 6.6818 VA/lb
@Magnetic Field 0.200 T,
Frequency 2500 Hz
6.6818 VA/lb
@Magnetic Field 0.200 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 6.9091 VA/lb
@Magnetic Field 1.40 T,
Frequency 100 Hz
6.9091 VA/lb
@Magnetic Field 1.40 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 7.00 VA/lb
@Magnetic Field 1.30 T,
Frequency 200 Hz
7.00 VA/lb
@Magnetic Field 1.30 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 7.5455 VA/lb
@Magnetic Field 1.00 T,
Frequency 400 Hz
7.5455 VA/lb
@Magnetic Field 1.00 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 7.5909 VA/lb
@Magnetic Field 1.40 T,
Frequency 100 Hz
7.5909 VA/lb
@Magnetic Field 1.40 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 8.3182 VA/lb
@Magnetic Field 1.30 T,
Frequency 200 Hz
8.3182 VA/lb
@Magnetic Field 1.30 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 8.4545 VA/lb
@Magnetic Field 1.00 T,
Frequency 400 Hz
8.4545 VA/lb
@Magnetic Field 1.00 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 8.50 VA/lb
@Magnetic Field 0.700 T,
Frequency 700 Hz
8.50 VA/lb
@Magnetic Field 0.700 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 9.2727 VA/lb
@Magnetic Field 0.700 T,
Frequency 700 Hz
9.2727 VA/lb
@Magnetic Field 0.700 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 10.0909 VA/lb
@Magnetic Field 0.400 T,
Frequency 1500 Hz
10.0909 VA/lb
@Magnetic Field 0.400 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 10.4545 VA/lb
@Magnetic Field 0.400 T,
Frequency 1500 Hz
10.4545 VA/lb
@Magnetic Field 0.400 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 11.0 VA/lb
@Magnetic Field 1.50 T,
Frequency 50 Hz
11.0 VA/lb
@Magnetic Field 1.50 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 11.5909 VA/lb
@Magnetic Field 1.20 T,
Frequency 400 Hz
11.5909 VA/lb
@Magnetic Field 1.20 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 11.6364 VA/lb
@Magnetic Field 1.50 T,
Frequency 50 Hz
11.6364 VA/lb
@Magnetic Field 1.50 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 13.2273 VA/lb
@Magnetic Field 1.20 T,
Frequency 400 Hz
13.2273 VA/lb
@Magnetic Field 1.20 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 13.3636 VA/lb
@Magnetic Field 1.50 T,
Frequency 60 Hz
13.3636 VA/lb
@Magnetic Field 1.50 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 13.8182 VA/lb
@Magnetic Field 0.700 T,
Frequency 1000 Hz
13.8182 VA/lb
@Magnetic Field 0.700 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 14.0909 VA/lb
@Magnetic Field 1.50 T,
Frequency 60 Hz
14.0909 VA/lb
@Magnetic Field 1.50 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 14.1364 VA/lb
@Magnetic Field 1.40 T,
Frequency 200 Hz
14.1364 VA/lb
@Magnetic Field 1.40 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 15.3636 VA/lb
@Magnetic Field 0.700 T,
Frequency 1000 Hz
15.3636 VA/lb
@Magnetic Field 0.700 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 15.5 VA/lb
@Magnetic Field 1.40 T,
Frequency 200 Hz
15.5 VA/lb
@Magnetic Field 1.40 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 15.8182 VA/lb
@Magnetic Field 1.30 T,
Frequency 400 Hz
15.8182 VA/lb
@Magnetic Field 1.30 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 16.5909 VA/lb
@Magnetic Field 1.00 T,
Frequency 700 Hz
16.5909 VA/lb
@Magnetic Field 1.00 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 16.7273 VA/lb
@Magnetic Field 0.100 T,
Frequency 10000 Hz
16.7273 VA/lb
@Magnetic Field 0.100 T,
Frequency 10000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 16.7727 VA/lb
@Magnetic Field 0.100 T,
Frequency 10000 Hz
16.7727 VA/lb
@Magnetic Field 0.100 T,
Frequency 10000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 18.0455 VA/lb
@Magnetic Field 1.00 T,
Frequency 700 Hz
18.0455 VA/lb
@Magnetic Field 1.00 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 18.1364 VA/lb
@Magnetic Field 1.30 T,
Frequency 400 Hz
18.1364 VA/lb
@Magnetic Field 1.30 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 19.1818 VA/lb
@Magnetic Field 0.200 T,
Frequency 5000 Hz
19.1818 VA/lb
@Magnetic Field 0.200 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 19.6364 VA/lb
@Magnetic Field 0.200 T,
Frequency 5000 Hz
19.6364 VA/lb
@Magnetic Field 0.200 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 21.7273 VA/lb
@Magnetic Field 0.400 T,
Frequency 2500 Hz
21.7273 VA/lb
@Magnetic Field 0.400 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 22.0 VA/lb
@Magnetic Field 0.400 T,
Frequency 2500 Hz
22.0 VA/lb
@Magnetic Field 0.400 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 22.2727 VA/lb
@Magnetic Field 1.50 T,
Frequency 100 Hz
22.2727 VA/lb
@Magnetic Field 1.50 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 24.5455 VA/lb
@Magnetic Field 1.50 T,
Frequency 100 Hz
24.5455 VA/lb
@Magnetic Field 1.50 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 25.2727 VA/lb
@Magnetic Field 1.20 T,
Frequency 700 Hz
25.2727 VA/lb
@Magnetic Field 1.20 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 27.0 VA/lb
@Magnetic Field 0.700 T,
Frequency 1500 Hz
27.0 VA/lb
@Magnetic Field 0.700 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 27.5455 VA/lb
@Magnetic Field 1.00 T,
Frequency 1000 Hz
27.5455 VA/lb
@Magnetic Field 1.00 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 27.7273 VA/lb
@Magnetic Field 0.700 T,
Frequency 1500 Hz
27.7273 VA/lb
@Magnetic Field 0.700 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 27.7273 VA/lb
@Magnetic Field 1.20 T,
Frequency 700 Hz
27.7273 VA/lb
@Magnetic Field 1.20 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 30.0455 VA/lb
@Magnetic Field 1.40 T,
Frequency 400 Hz
30.0455 VA/lb
@Magnetic Field 1.40 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 30.3182 VA/lb
@Magnetic Field 1.00 T,
Frequency 1000 Hz
30.3182 VA/lb
@Magnetic Field 1.00 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 31.0 VA/lb
@Magnetic Field 1.60 T,
Frequency 50 Hz
31.0 VA/lb
@Magnetic Field 1.60 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 32.3636 VA/lb
@Magnetic Field 1.40 T,
Frequency 400 Hz
32.3636 VA/lb
@Magnetic Field 1.40 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 33.1818 VA/lb
@Magnetic Field 1.30 T,
Frequency 700 Hz
33.1818 VA/lb
@Magnetic Field 1.30 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 33.3636 VA/lb
@Magnetic Field 1.60 T,
Frequency 50 Hz
33.3636 VA/lb
@Magnetic Field 1.60 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 37.0455 VA/lb
@Magnetic Field 1.30 T,
Frequency 700 Hz
37.0455 VA/lb
@Magnetic Field 1.30 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 37.5 VA/lb
@Magnetic Field 1.60 T,
Frequency 60 Hz
37.5 VA/lb
@Magnetic Field 1.60 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 40.3636 VA/lb
@Magnetic Field 1.60 T,
Frequency 60 Hz
40.3636 VA/lb
@Magnetic Field 1.60 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 41.5 VA/lb
@Magnetic Field 1.20 T,
Frequency 1000 Hz
41.5 VA/lb
@Magnetic Field 1.20 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 44.8182 VA/lb
@Magnetic Field 1.50 T,
Frequency 200 Hz
44.8182 VA/lb
@Magnetic Field 1.50 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 46.3636 VA/lb
@Magnetic Field 1.20 T,
Frequency 1000 Hz
46.3636 VA/lb
@Magnetic Field 1.20 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 49.5455 VA/lb
@Magnetic Field 1.50 T,
Frequency 200 Hz
49.5455 VA/lb
@Magnetic Field 1.50 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 52.7273 VA/lb
@Magnetic Field 1.30 T,
Frequency 1000 Hz
52.7273 VA/lb
@Magnetic Field 1.30 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 55.0 VA/lb
@Magnetic Field 1.00 T,
Frequency 1500 Hz
55.0 VA/lb
@Magnetic Field 1.00 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 56.3636 VA/lb
@Magnetic Field 1.00 T,
Frequency 1500 Hz
56.3636 VA/lb
@Magnetic Field 1.00 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 56.8182 VA/lb
@Magnetic Field 0.200 T,
Frequency 10000 Hz
56.8182 VA/lb
@Magnetic Field 0.200 T,
Frequency 10000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 57.2727 VA/lb
@Magnetic Field 0.200 T,
Frequency 10000 Hz
57.2727 VA/lb
@Magnetic Field 0.200 T,
Frequency 10000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 60.0 VA/lb
@Magnetic Field 0.700 T,
Frequency 2500 Hz
60.0 VA/lb
@Magnetic Field 0.700 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 60.4545 VA/lb
@Magnetic Field 1.30 T,
Frequency 1000 Hz
60.4545 VA/lb
@Magnetic Field 1.30 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 60.9091 VA/lb
@Magnetic Field 0.700 T,
Frequency 2500 Hz
60.9091 VA/lb
@Magnetic Field 0.700 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 62.2727 VA/lb
@Magnetic Field 1.60 T,
Frequency 100 Hz
62.2727 VA/lb
@Magnetic Field 1.60 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 63.6364 VA/lb
@Magnetic Field 0.400 T,
Frequency 5000 Hz
63.6364 VA/lb
@Magnetic Field 0.400 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 65.0 VA/lb
@Magnetic Field 0.400 T,
Frequency 5000 Hz
65.0 VA/lb
@Magnetic Field 0.400 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 68.1818 VA/lb
@Magnetic Field 1.70 T,
Frequency 50 Hz
68.1818 VA/lb
@Magnetic Field 1.70 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 69.5455 VA/lb
@Magnetic Field 1.60 T,
Frequency 100 Hz
69.5455 VA/lb
@Magnetic Field 1.60 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 71.8182 VA/lb
@Magnetic Field 1.70 T,
Frequency 50 Hz
71.8182 VA/lb
@Magnetic Field 1.70 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 82.2727 VA/lb
@Magnetic Field 1.70 T,
Frequency 60 Hz
82.2727 VA/lb
@Magnetic Field 1.70 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 84.5455 VA/lb
@Magnetic Field 1.20 T,
Frequency 1500 Hz
84.5455 VA/lb
@Magnetic Field 1.20 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 86.3636 VA/lb
@Magnetic Field 1.20 T,
Frequency 1500 Hz
86.3636 VA/lb
@Magnetic Field 1.20 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 86.8182 VA/lb
@Magnetic Field 1.70 T,
Frequency 60 Hz
86.8182 VA/lb
@Magnetic Field 1.70 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 92.2727 VA/lb
@Magnetic Field 1.50 T,
Frequency 400 Hz
92.2727 VA/lb
@Magnetic Field 1.50 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 102.73 VA/lb
@Magnetic Field 1.50 T,
Frequency 400 Hz
102.73 VA/lb
@Magnetic Field 1.50 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 107.27 VA/lb
@Magnetic Field 1.30 T,
Frequency 1500 Hz
107.27 VA/lb
@Magnetic Field 1.30 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 110 VA/lb
@Magnetic Field 1.30 T,
Frequency 1500 Hz
110 VA/lb
@Magnetic Field 1.30 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 125.45 VA/lb
@Magnetic Field 1.60 T,
Frequency 200 Hz
125.45 VA/lb
@Magnetic Field 1.60 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 129.09 VA/lb
@Magnetic Field 1.00 T,
Frequency 2500 Hz
129.09 VA/lb
@Magnetic Field 1.00 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 129.55 VA/lb
@Magnetic Field 1.00 T,
Frequency 2500 Hz
129.55 VA/lb
@Magnetic Field 1.00 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 136.86 VA/lb
@Magnetic Field 1.70 T,
Frequency 100 Hz
136.86 VA/lb
@Magnetic Field 1.70 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 139.55 VA/lb
@Magnetic Field 1.60 T,
Frequency 200 Hz
139.55 VA/lb
@Magnetic Field 1.60 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 148.18 VA/lb
@Magnetic Field 1.70 T,
Frequency 100 Hz
148.18 VA/lb
@Magnetic Field 1.70 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 189.09 VA/lb
@Magnetic Field 0.700 T,
Frequency 5000 Hz
189.09 VA/lb
@Magnetic Field 0.700 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 193.18 VA/lb
@Magnetic Field 0.700 T,
Frequency 5000 Hz
193.18 VA/lb
@Magnetic Field 0.700 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 195 VA/lb
@Magnetic Field 0.400 T,
Frequency 10000 Hz
195 VA/lb
@Magnetic Field 0.400 T,
Frequency 10000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 196.36 VA/lb
@Magnetic Field 0.400 T,
Frequency 10000 Hz
196.36 VA/lb
@Magnetic Field 0.400 T,
Frequency 10000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 201.82 VA/lb
@Magnetic Field 1.20 T,
Frequency 2500 Hz
201.82 VA/lb
@Magnetic Field 1.20 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 254.09 VA/lb
@Magnetic Field 1.30 T,
Frequency 2500 Hz
254.09 VA/lb
@Magnetic Field 1.30 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 260.91 VA/lb
@Magnetic Field 1.60 T,
Frequency 400 Hz
260.91 VA/lb
@Magnetic Field 1.60 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 274.55 VA/lb
@Magnetic Field 1.70 T,
Frequency 200 Hz
274.55 VA/lb
@Magnetic Field 1.70 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 289.09 VA/lb
@Magnetic Field 1.60 T,
Frequency 400 Hz
289.09 VA/lb
@Magnetic Field 1.60 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 297.27 VA/lb
@Magnetic Field 1.70 T,
Frequency 200 Hz
297.27 VA/lb
@Magnetic Field 1.70 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 434.55 VA/lb
@Magnetic Field 1.00 T,
Frequency 5000 Hz
434.55 VA/lb
@Magnetic Field 1.00 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 438.64 VA/lb
@Magnetic Field 1.00 T,
Frequency 5000 Hz
438.64 VA/lb
@Magnetic Field 1.00 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
Electrical Resistivity 0.0000540 - 0.0000560 ohm-cm0.0000540 - 0.0000560 ohm-cm
 
Magnetic PropertiesMetricEnglishComments
Core Loss  0.0123 W/kg
@Magnetic Field 0.100 T,
Frequency 50 Hz
0.00558 W/lb
@Magnetic Field 0.100 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.0125 W/kg
@Magnetic Field 0.100 T,
Frequency 50 Hz
0.00567 W/lb
@Magnetic Field 0.100 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.0151 W/kg
@Magnetic Field 0.100 T,
Frequency 60 Hz
0.00685 W/lb
@Magnetic Field 0.100 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.0153 W/kg
@Magnetic Field 0.100 T,
Frequency 60 Hz
0.00694 W/lb
@Magnetic Field 0.100 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.0271 W/kg
@Magnetic Field 0.100 T,
Frequency 100 Hz
0.0123 W/lb
@Magnetic Field 0.100 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.0279 W/kg
@Magnetic Field 0.100 T,
Frequency 100 Hz
0.0127 W/lb
@Magnetic Field 0.100 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.0498 W/kg
@Magnetic Field 0.200 T,
Frequency 50 Hz
0.0226 W/lb
@Magnetic Field 0.200 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.0556 W/kg
@Magnetic Field 0.200 T,
Frequency 50 Hz
0.0252 W/lb
@Magnetic Field 0.200 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.0613 W/kg
@Magnetic Field 0.200 T,
Frequency 60 Hz
0.0278 W/lb
@Magnetic Field 0.200 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.0648 W/kg
@Magnetic Field 0.100 T,
Frequency 200 Hz
0.0294 W/lb
@Magnetic Field 0.100 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.0671 W/kg
@Magnetic Field 0.100 T,
Frequency 200 Hz
0.0304 W/lb
@Magnetic Field 0.100 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.0683 W/kg
@Magnetic Field 0.200 T,
Frequency 60 Hz
0.0310 W/lb
@Magnetic Field 0.200 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.112 W/kg
@Magnetic Field 0.200 T,
Frequency 100 Hz
0.0508 W/lb
@Magnetic Field 0.200 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.123 W/kg
@Magnetic Field 0.200 T,
Frequency 100 Hz
0.0558 W/lb
@Magnetic Field 0.200 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.170 W/kg
@Magnetic Field 0.100 T,
Frequency 400 Hz
0.0771 W/lb
@Magnetic Field 0.100 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.177 W/kg
@Magnetic Field 0.100 T,
Frequency 400 Hz
0.0803 W/lb
@Magnetic Field 0.100 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.179 W/kg
@Magnetic Field 0.400 T,
Frequency 50 Hz
0.0812 W/lb
@Magnetic Field 0.400 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.205 W/kg
@Magnetic Field 0.400 T,
Frequency 50 Hz
0.0930 W/lb
@Magnetic Field 0.400 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.221 W/kg
@Magnetic Field 0.400 T,
Frequency 60 Hz
0.100 W/lb
@Magnetic Field 0.400 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.252 W/kg
@Magnetic Field 0.400 T,
Frequency 60 Hz
0.114 W/lb
@Magnetic Field 0.400 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.269 W/kg
@Magnetic Field 0.200 T,
Frequency 200 Hz
0.122 W/lb
@Magnetic Field 0.200 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.289 W/kg
@Magnetic Field 0.200 T,
Frequency 200 Hz
0.131 W/lb
@Magnetic Field 0.200 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.396 W/kg
@Magnetic Field 0.100 T,
Frequency 700 Hz
0.180 W/lb
@Magnetic Field 0.100 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.409 W/kg
@Magnetic Field 0.400 T,
Frequency 100 Hz
0.186 W/lb
@Magnetic Field 0.400 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.415 W/kg
@Magnetic Field 0.100 T,
Frequency 700 Hz
0.188 W/lb
@Magnetic Field 0.100 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.460 W/kg
@Magnetic Field 0.400 T,
Frequency 100 Hz
0.209 W/lb
@Magnetic Field 0.400 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.467 W/kg
@Magnetic Field 0.700 T,
Frequency 50 Hz
0.212 W/lb
@Magnetic Field 0.700 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.528 W/kg
@Magnetic Field 0.700 T,
Frequency 50 Hz
0.239 W/lb
@Magnetic Field 0.700 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.578 W/kg
@Magnetic Field 0.700 T,
Frequency 60 Hz
0.262 W/lb
@Magnetic Field 0.700 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.651 W/kg
@Magnetic Field 0.700 T,
Frequency 60 Hz
0.295 W/lb
@Magnetic Field 0.700 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.699 W/kg
@Magnetic Field 0.100 T,
Frequency 1000 Hz
0.317 W/lb
@Magnetic Field 0.100 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.703 W/kg
@Magnetic Field 0.200 T,
Frequency 400 Hz
0.319 W/lb
@Magnetic Field 0.200 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.730 W/kg
@Magnetic Field 0.100 T,
Frequency 1000 Hz
0.331 W/lb
@Magnetic Field 0.100 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.736 W/kg
@Magnetic Field 0.200 T,
Frequency 400 Hz
0.334 W/lb
@Magnetic Field 0.200 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.873 W/kg
@Magnetic Field 1.00 T,
Frequency 50 Hz
0.396 W/lb
@Magnetic Field 1.00 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 0.972 W/kg
@Magnetic Field 1.00 T,
Frequency 50 Hz
0.441 W/lb
@Magnetic Field 1.00 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 0.994 W/kg
@Magnetic Field 0.400 T,
Frequency 200 Hz
0.451 W/lb
@Magnetic Field 0.400 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 1.08 W/kg
@Magnetic Field 1.00 T,
Frequency 60 Hz
0.490 W/lb
@Magnetic Field 1.00 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 1.09 W/kg
@Magnetic Field 0.400 T,
Frequency 200 Hz
0.494 W/lb
@Magnetic Field 0.400 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 1.09 W/kg
@Magnetic Field 0.700 T,
Frequency 100 Hz
0.494 W/lb
@Magnetic Field 0.700 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 1.20 W/kg
@Magnetic Field 0.700 T,
Frequency 100 Hz
0.544 W/lb
@Magnetic Field 0.700 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 1.20 W/kg
@Magnetic Field 1.00 T,
Frequency 60 Hz
0.544 W/lb
@Magnetic Field 1.00 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 1.26 W/kg
@Magnetic Field 1.20 T,
Frequency 50 Hz
0.572 W/lb
@Magnetic Field 1.20 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 1.36 W/kg
@Magnetic Field 0.100 T,
Frequency 1500 Hz
0.617 W/lb
@Magnetic Field 0.100 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 1.38 W/kg
@Magnetic Field 1.20 T,
Frequency 50 Hz
0.626 W/lb
@Magnetic Field 1.20 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 1.41 W/kg
@Magnetic Field 0.100 T,
Frequency 1500 Hz
0.640 W/lb
@Magnetic Field 0.100 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 1.54 W/kg
@Magnetic Field 1.30 T,
Frequency 50 Hz
0.699 W/lb
@Magnetic Field 1.30 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 1.57 W/kg
@Magnetic Field 1.20 T,
Frequency 60 Hz
0.712 W/lb
@Magnetic Field 1.20 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 1.62 W/kg
@Magnetic Field 0.200 T,
Frequency 700 Hz
0.735 W/lb
@Magnetic Field 0.200 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 1.66 W/kg
@Magnetic Field 0.200 T,
Frequency 700 Hz
0.753 W/lb
@Magnetic Field 0.200 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 1.66 W/kg
@Magnetic Field 1.30 T,
Frequency 50 Hz
0.753 W/lb
@Magnetic Field 1.30 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 1.71 W/kg
@Magnetic Field 1.20 T,
Frequency 60 Hz
0.776 W/lb
@Magnetic Field 1.20 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 1.91 W/kg
@Magnetic Field 1.30 T,
Frequency 60 Hz
0.866 W/lb
@Magnetic Field 1.30 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 1.93 W/kg
@Magnetic Field 1.40 T,
Frequency 50 Hz
0.875 W/lb
@Magnetic Field 1.40 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 2.02 W/kg
@Magnetic Field 1.40 T,
Frequency 50 Hz
0.916 W/lb
@Magnetic Field 1.40 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 2.04 W/kg
@Magnetic Field 1.00 T,
Frequency 100 Hz
0.925 W/lb
@Magnetic Field 1.00 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 2.05 W/kg
@Magnetic Field 1.30 T,
Frequency 60 Hz
0.930 W/lb
@Magnetic Field 1.30 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 2.22 W/kg
@Magnetic Field 1.00 T,
Frequency 100 Hz
1.01 W/lb
@Magnetic Field 1.00 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 2.39 W/kg
@Magnetic Field 1.40 T,
Frequency 60 Hz
1.08 W/lb
@Magnetic Field 1.40 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 2.42 W/kg
@Magnetic Field 1.50 T,
Frequency 50 Hz
1.10 W/lb
@Magnetic Field 1.50 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 2.45 W/kg
@Magnetic Field 1.50 T,
Frequency 50 Hz
1.11 W/lb
@Magnetic Field 1.50 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 2.49 W/kg
@Magnetic Field 1.40 T,
Frequency 60 Hz
1.13 W/lb
@Magnetic Field 1.40 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 2.60 W/kg
@Magnetic Field 0.400 T,
Frequency 400 Hz
1.18 W/lb
@Magnetic Field 0.400 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 2.69 W/kg
@Magnetic Field 0.700 T,
Frequency 200 Hz
1.22 W/lb
@Magnetic Field 0.700 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 2.78 W/kg
@Magnetic Field 0.400 T,
Frequency 400 Hz
1.26 W/lb
@Magnetic Field 0.400 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 2.82 W/kg
@Magnetic Field 0.200 T,
Frequency 1000 Hz
1.28 W/lb
@Magnetic Field 0.200 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 2.86 W/kg
@Magnetic Field 0.200 T,
Frequency 1000 Hz
1.30 W/lb
@Magnetic Field 0.200 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 2.87 W/kg
@Magnetic Field 1.60 T,
Frequency 50 Hz
1.30 W/lb
@Magnetic Field 1.60 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 2.88 W/kg
@Magnetic Field 1.60 T,
Frequency 50 Hz
1.31 W/lb
@Magnetic Field 1.60 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 2.91 W/kg
@Magnetic Field 0.700 T,
Frequency 200 Hz
1.32 W/lb
@Magnetic Field 0.700 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 2.94 W/kg
@Magnetic Field 1.20 T,
Frequency 100 Hz
1.33 W/lb
@Magnetic Field 1.20 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 2.99 W/kg
@Magnetic Field 1.50 T,
Frequency 60 Hz
1.36 W/lb
@Magnetic Field 1.50 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 3.03 W/kg
@Magnetic Field 1.50 T,
Frequency 60 Hz
1.37 W/lb
@Magnetic Field 1.50 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 3.16 W/kg
@Magnetic Field 1.20 T,
Frequency 100 Hz
1.43 W/lb
@Magnetic Field 1.20 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 3.23 W/kg
@Magnetic Field 0.100 T,
Frequency 2500 Hz
1.47 W/lb
@Magnetic Field 0.100 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 3.25 W/kg
@Magnetic Field 1.70 T,
Frequency 50 Hz
1.47 W/lb
@Magnetic Field 1.70 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 3.28 W/kg
@Magnetic Field 1.70 T,
Frequency 50 Hz
1.49 W/lb
@Magnetic Field 1.70 T,
Frequency 50 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 3.32 W/kg
@Magnetic Field 0.100 T,
Frequency 2500 Hz
1.51 W/lb
@Magnetic Field 0.100 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 3.54 W/kg
@Magnetic Field 1.60 T,
Frequency 60 Hz
1.61 W/lb
@Magnetic Field 1.60 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 3.56 W/kg
@Magnetic Field 1.60 T,
Frequency 60 Hz
1.61 W/lb
@Magnetic Field 1.60 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 3.58 W/kg
@Magnetic Field 1.30 T,
Frequency 100 Hz
1.62 W/lb
@Magnetic Field 1.30 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 3.78 W/kg
@Magnetic Field 1.30 T,
Frequency 100 Hz
1.71 W/lb
@Magnetic Field 1.30 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 4.00 W/kg
@Magnetic Field 1.70 T,
Frequency 60 Hz
1.81 W/lb
@Magnetic Field 1.70 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 4.05 W/kg
@Magnetic Field 1.70 T,
Frequency 60 Hz
1.84 W/lb
@Magnetic Field 1.70 T,
Frequency 60 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 4.46 W/kg
@Magnetic Field 1.40 T,
Frequency 100 Hz
2.02 W/lb
@Magnetic Field 1.40 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 4.58 W/kg
@Magnetic Field 1.40 T,
Frequency 100 Hz
2.08 W/lb
@Magnetic Field 1.40 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 5.09 W/kg
@Magnetic Field 1.00 T,
Frequency 200 Hz
2.31 W/lb
@Magnetic Field 1.00 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 5.38 W/kg
@Magnetic Field 0.200 T,
Frequency 1500 Hz
2.44 W/lb
@Magnetic Field 0.200 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 5.43 W/kg
@Magnetic Field 0.200 T,
Frequency 1500 Hz
2.46 W/lb
@Magnetic Field 0.200 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 5.43 W/kg
@Magnetic Field 1.00 T,
Frequency 200 Hz
2.46 W/lb
@Magnetic Field 1.00 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 5.53 W/kg
@Magnetic Field 1.50 T,
Frequency 100 Hz
2.51 W/lb
@Magnetic Field 1.50 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 5.57 W/kg
@Magnetic Field 1.50 T,
Frequency 100 Hz
2.53 W/lb
@Magnetic Field 1.50 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 5.96 W/kg
@Magnetic Field 0.400 T,
Frequency 700 Hz
2.70 W/lb
@Magnetic Field 0.400 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 6.23 W/kg
@Magnetic Field 0.400 T,
Frequency 700 Hz
2.83 W/lb
@Magnetic Field 0.400 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 6.47 W/kg
@Magnetic Field 1.60 T,
Frequency 100 Hz
2.93 W/lb
@Magnetic Field 1.60 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 6.67 W/kg
@Magnetic Field 1.60 T,
Frequency 100 Hz
3.03 W/lb
@Magnetic Field 1.60 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 7.14 W/kg
@Magnetic Field 0.700 T,
Frequency 400 Hz
3.24 W/lb
@Magnetic Field 0.700 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 7.23 W/kg
@Magnetic Field 1.70 T,
Frequency 100 Hz
3.28 W/lb
@Magnetic Field 1.70 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 7.30 W/kg
@Magnetic Field 1.20 T,
Frequency 200 Hz
3.31 W/lb
@Magnetic Field 1.20 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 7.47 W/kg
@Magnetic Field 1.70 T,
Frequency 100 Hz
3.39 W/lb
@Magnetic Field 1.70 T,
Frequency 100 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 7.55 W/kg
@Magnetic Field 0.700 T,
Frequency 400 Hz
3.42 W/lb
@Magnetic Field 0.700 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 7.70 W/kg
@Magnetic Field 1.20 T,
Frequency 200 Hz
3.49 W/lb
@Magnetic Field 1.20 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 8.83 W/kg
@Magnetic Field 1.30 T,
Frequency 200 Hz
4.01 W/lb
@Magnetic Field 1.30 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 9.18 W/kg
@Magnetic Field 1.30 T,
Frequency 200 Hz
4.16 W/lb
@Magnetic Field 1.30 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 10.3 W/kg
@Magnetic Field 0.400 T,
Frequency 1000 Hz
4.67 W/lb
@Magnetic Field 0.400 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 10.4 W/kg
@Magnetic Field 0.100 T,
Frequency 5000 Hz
4.72 W/lb
@Magnetic Field 0.100 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 10.6 W/kg
@Magnetic Field 0.400 T,
Frequency 1000 Hz
4.81 W/lb
@Magnetic Field 0.400 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 10.6 W/kg
@Magnetic Field 0.100 T,
Frequency 5000 Hz
4.81 W/lb
@Magnetic Field 0.100 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 10.9 W/kg
@Magnetic Field 1.40 T,
Frequency 200 Hz
4.94 W/lb
@Magnetic Field 1.40 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 11.1 W/kg
@Magnetic Field 1.40 T,
Frequency 200 Hz
5.03 W/lb
@Magnetic Field 1.40 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 12.3 W/kg
@Magnetic Field 0.200 T,
Frequency 2500 Hz
5.58 W/lb
@Magnetic Field 0.200 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 12.4 W/kg
@Magnetic Field 0.200 T,
Frequency 2500 Hz
5.62 W/lb
@Magnetic Field 0.200 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 13.3 W/kg
@Magnetic Field 1.50 T,
Frequency 200 Hz
6.03 W/lb
@Magnetic Field 1.50 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 13.5 W/kg
@Magnetic Field 1.50 T,
Frequency 200 Hz
6.12 W/lb
@Magnetic Field 1.50 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 13.7 W/kg
@Magnetic Field 1.00 T,
Frequency 400 Hz
6.21 W/lb
@Magnetic Field 1.00 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 13.7 W/kg
@Magnetic Field 1.00 T,
Frequency 400 Hz
6.21 W/lb
@Magnetic Field 1.00 T,
Frequency 400 Hz
Typical, After 830°C Stress Relief Annealed
 14.4 W/kg
@Magnetic Field 1.00 T,
Frequency 400 Hz
6.53 W/lb
@Magnetic Field 1.00 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 14.5 W/kg
@Magnetic Field 1.00 T,
Frequency 400 Hz
6.58 W/lb
@Magnetic Field 1.00 T,
Frequency 400 Hz
Typical, As Sheared
 <= 14.5 W/kg
@Magnetic Field 1.00 T,
Frequency 400 Hz
<= 6.58 W/lb
@Magnetic Field 1.00 T,
Frequency 400 Hz
After 830°C Stress Relief Annealed
 15.5 W/kg
@Magnetic Field 1.60 T,
Frequency 200 Hz
7.03 W/lb
@Magnetic Field 1.60 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 15.5 W/kg
@Magnetic Field 1.00 T,
Frequency 400 Hz
7.03 W/lb
@Magnetic Field 1.00 T,
Frequency 400 Hz
Maximum, As Sheared
 16.0 W/kg
@Magnetic Field 1.60 T,
Frequency 200 Hz
7.26 W/lb
@Magnetic Field 1.60 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 16.5 W/kg
@Magnetic Field 0.700 T,
Frequency 700 Hz
7.48 W/lb
@Magnetic Field 0.700 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 17.1 W/kg
@Magnetic Field 0.700 T,
Frequency 700 Hz
7.76 W/lb
@Magnetic Field 0.700 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 17.1 W/kg
@Magnetic Field 1.70 T,
Frequency 200 Hz
7.76 W/lb
@Magnetic Field 1.70 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 17.7 W/kg
@Magnetic Field 1.70 T,
Frequency 200 Hz
8.03 W/lb
@Magnetic Field 1.70 T,
Frequency 200 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 19.4 W/kg
@Magnetic Field 0.400 T,
Frequency 1500 Hz
8.80 W/lb
@Magnetic Field 0.400 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 19.8 W/kg
@Magnetic Field 0.400 T,
Frequency 1500 Hz
8.98 W/lb
@Magnetic Field 0.400 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 19.8 W/kg
@Magnetic Field 1.20 T,
Frequency 400 Hz
8.98 W/lb
@Magnetic Field 1.20 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 20.4 W/kg
@Magnetic Field 1.20 T,
Frequency 400 Hz
9.25 W/lb
@Magnetic Field 1.20 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 23.7 W/kg
@Magnetic Field 1.30 T,
Frequency 400 Hz
10.8 W/lb
@Magnetic Field 1.30 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 24.3 W/kg
@Magnetic Field 1.30 T,
Frequency 400 Hz
11.0 W/lb
@Magnetic Field 1.30 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 28.4 W/kg
@Magnetic Field 0.700 T,
Frequency 1000 Hz
12.9 W/lb
@Magnetic Field 0.700 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 29.0 W/kg
@Magnetic Field 1.40 T,
Frequency 400 Hz
13.2 W/lb
@Magnetic Field 1.40 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 29.0 W/kg
@Magnetic Field 1.40 T,
Frequency 400 Hz
13.2 W/lb
@Magnetic Field 1.40 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 29.4 W/kg
@Magnetic Field 0.700 T,
Frequency 1000 Hz
13.3 W/lb
@Magnetic Field 0.700 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 32.3 W/kg
@Magnetic Field 1.00 T,
Frequency 700 Hz
14.7 W/lb
@Magnetic Field 1.00 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 32.7 W/kg
@Magnetic Field 0.100 T,
Frequency 10000 Hz
14.8 W/lb
@Magnetic Field 0.100 T,
Frequency 10000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 33.4 W/kg
@Magnetic Field 1.00 T,
Frequency 700 Hz
15.1 W/lb
@Magnetic Field 1.00 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 33.5 W/kg
@Magnetic Field 0.100 T,
Frequency 10000 Hz
15.2 W/lb
@Magnetic Field 0.100 T,
Frequency 10000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 35.0 W/kg
@Magnetic Field 1.50 T,
Frequency 400 Hz
15.9 W/lb
@Magnetic Field 1.50 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 35.7 W/kg
@Magnetic Field 1.50 T,
Frequency 400 Hz
16.2 W/lb
@Magnetic Field 1.50 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 37.5 W/kg
@Magnetic Field 0.200 T,
Frequency 5000 Hz
17.0 W/lb
@Magnetic Field 0.200 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 37.9 W/kg
@Magnetic Field 0.200 T,
Frequency 5000 Hz
17.2 W/lb
@Magnetic Field 0.200 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 40.1 W/kg
@Magnetic Field 1.60 T,
Frequency 400 Hz
18.2 W/lb
@Magnetic Field 1.60 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 41.3 W/kg
@Magnetic Field 1.60 T,
Frequency 400 Hz
18.7 W/lb
@Magnetic Field 1.60 T,
Frequency 400 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 43.0 W/kg
@Magnetic Field 0.400 T,
Frequency 2500 Hz
19.5 W/lb
@Magnetic Field 0.400 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 43.8 W/kg
@Magnetic Field 0.400 T,
Frequency 2500 Hz
19.9 W/lb
@Magnetic Field 0.400 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 47.3 W/kg
@Magnetic Field 1.20 T,
Frequency 700 Hz
21.5 W/lb
@Magnetic Field 1.20 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 48.3 W/kg
@Magnetic Field 1.20 T,
Frequency 700 Hz
21.9 W/lb
@Magnetic Field 1.20 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 53.3 W/kg
@Magnetic Field 0.700 T,
Frequency 1500 Hz
24.2 W/lb
@Magnetic Field 0.700 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 55.3 W/kg
@Magnetic Field 0.700 T,
Frequency 1500 Hz
25.1 W/lb
@Magnetic Field 0.700 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 56.7 W/kg
@Magnetic Field 1.00 T,
Frequency 1000 Hz
25.7 W/lb
@Magnetic Field 1.00 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 56.7 W/kg
@Magnetic Field 1.30 T,
Frequency 700 Hz
25.7 W/lb
@Magnetic Field 1.30 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 56.9 W/kg
@Magnetic Field 1.30 T,
Frequency 700 Hz
25.8 W/lb
@Magnetic Field 1.30 T,
Frequency 700 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 58.3 W/kg
@Magnetic Field 1.00 T,
Frequency 1000 Hz
26.4 W/lb
@Magnetic Field 1.00 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 84.1 W/kg
@Magnetic Field 1.20 T,
Frequency 1000 Hz
38.1 W/lb
@Magnetic Field 1.20 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 85.2 W/kg
@Magnetic Field 1.20 T,
Frequency 1000 Hz
38.6 W/lb
@Magnetic Field 1.20 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 101.1 W/kg
@Magnetic Field 1.30 T,
Frequency 1000 Hz
45.86 W/lb
@Magnetic Field 1.30 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 102 W/kg
@Magnetic Field 1.30 T,
Frequency 1000 Hz
46.3 W/lb
@Magnetic Field 1.30 T,
Frequency 1000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 109 W/kg
@Magnetic Field 1.00 T,
Frequency 1500 Hz
49.4 W/lb
@Magnetic Field 1.00 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 112 W/kg
@Magnetic Field 1.00 T,
Frequency 1500 Hz
50.8 W/lb
@Magnetic Field 1.00 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 113 W/kg
@Magnetic Field 0.200 T,
Frequency 10000 Hz
51.3 W/lb
@Magnetic Field 0.200 T,
Frequency 10000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 115 W/kg
@Magnetic Field 0.200 T,
Frequency 10000 Hz
52.2 W/lb
@Magnetic Field 0.200 T,
Frequency 10000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 121 W/kg
@Magnetic Field 0.700 T,
Frequency 2500 Hz
54.9 W/lb
@Magnetic Field 0.700 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 125 W/kg
@Magnetic Field 0.700 T,
Frequency 2500 Hz
56.7 W/lb
@Magnetic Field 0.700 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 128 W/kg
@Magnetic Field 0.400 T,
Frequency 5000 Hz
58.1 W/lb
@Magnetic Field 0.400 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 128 W/kg
@Magnetic Field 0.400 T,
Frequency 5000 Hz
58.1 W/lb
@Magnetic Field 0.400 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 164 W/kg
@Magnetic Field 1.20 T,
Frequency 1500 Hz
74.4 W/lb
@Magnetic Field 1.20 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 168 W/kg
@Magnetic Field 1.20 T,
Frequency 1500 Hz
76.2 W/lb
@Magnetic Field 1.20 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 200 W/kg
@Magnetic Field 1.30 T,
Frequency 1500 Hz
90.7 W/lb
@Magnetic Field 1.30 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 200 W/kg
@Magnetic Field 1.30 T,
Frequency 1500 Hz
90.7 W/lb
@Magnetic Field 1.30 T,
Frequency 1500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 254 W/kg
@Magnetic Field 1.00 T,
Frequency 2500 Hz
115 W/lb
@Magnetic Field 1.00 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 265 W/kg
@Magnetic Field 1.00 T,
Frequency 2500 Hz
120 W/lb
@Magnetic Field 1.00 T,
Frequency 2500 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 380 W/kg
@Magnetic Field 0.700 T,
Frequency 5000 Hz
172 W/lb
@Magnetic Field 0.700 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 382 W/kg
@Magnetic Field 0.700 T,
Frequency 5000 Hz
173 W/lb
@Magnetic Field 0.700 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 395 W/kg
@Magnetic Field 0.400 T,
Frequency 10000 Hz
179 W/lb
@Magnetic Field 0.400 T,
Frequency 10000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 398 W/kg
@Magnetic Field 0.400 T,
Frequency 10000 Hz
181 W/lb
@Magnetic Field 0.400 T,
Frequency 10000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 842 W/kg
@Magnetic Field 1.00 T,
Frequency 5000 Hz
382 W/lb
@Magnetic Field 1.00 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, As-Sheared
 843 W/kg
@Magnetic Field 1.00 T,
Frequency 5000 Hz
382 W/lb
@Magnetic Field 1.00 T,
Frequency 5000 Hz
ASTM A343, ASTM A348, 50/50, Stress Relief Annealed
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 0.70 %0.70 %
Iron, Fe 96.65 %96.65 %As Balance
Silicon, Si 2.65 %2.65 %
 
Descriptive Properties
Magnetic Induction at 5000 A/m (T)1.65
Saturation Induction (T)1.99

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AK Steel DI-MAX® M-15 Nonoriented Electrical Steel
AK Steel DI-MAX® M-19 Nonoriented Electrical Steel
AK Steel CARLITE® M-6 Grain Oriented Electrical Steel (Extended Electro-Magnetic Data)
AK Steel DI-MAX® M-47 Nonoriented Electrical Steel
AK Steel DI-MAX® HF-10 Nonoriented Electrical Steel

NAKS162aa / 170643

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.