Physical Properties | Original Value | Comments |
---|
Density | 7.65 g/cc |
Thickness | 11.0 mil |
|
Mechanical Properties | Original Value | Comments |
---|
Hardness, Knoop | 167 |
Hardness, Rockwell B | 81 |
Tensile Strength, Ultimate | 51000 psi |
Tensile Strength, Yield | 48000 psi |
Elongation at Break | 9.0 % |
Modulus of Elasticity | 122 GPa |
| 143 GPa |
| 200 GPa |
| 236 GPa |
| 258 GPa |
|
Electrical Properties | Original Value | Comments |
---|
Exciting Power (RMS) | 0.00424 RMS VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00472 RMS VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00524 RMS VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00583 RMS VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.0141 RMS VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0154 RMS VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0176 RMS VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0192 RMS VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0283 RMS VA/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0305 RMS VA/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0354 RMS VA/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0381 RMS VA/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0457 RMS VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0488 RMS VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0574 RMS VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0613 RMS VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0659 RMS VA/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0699 RMS VA/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0831 RMS VA/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0881 RMS VA/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0887 RMS VA/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0937 RMS VA/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.112 RMS VA/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.114 RMS VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.118 RMS VA/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.120 RMS VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.142 RMS VA/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.145 RMS VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.149 RMS VA/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.152 RMS VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.173 RMS VA/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.181 RMS VA/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.181 RMS VA/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.189 RMS VA/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.208 RMS VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.218 RMS VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.221 RMS VA/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.231 RMS VA/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.248 RMS VA/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.258 RMS VA/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.265 RMS VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.277 RMS VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.294 RMS VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.306 RMS VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.316 RMS VA/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.329 RMS VA/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.351 RMS VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.365 RMS VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.374 RMS VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.389 RMS VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.424 RMS VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.437 RMS VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.445 RMS VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.463 RMS VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.533 RMS VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.537 RMS VA/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.552 RMS VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.553 RMS AT/cm @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.669 RMS VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.694 RMS VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.711 RMS VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.726 RMS VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.883 RMS VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.901 RMS VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 1.24 RMS VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 1.25 RMS VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 1.52 RMS VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.53 RMS VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 3.50 RMS VA/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 3.72 RMS VA/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 4.25 RMS VA/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 4.52 RMS VA/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 12.4 RMS VA/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 15.1 RMS VA/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
| 16.4 RMS VA/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 20.0 RMS VA/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
Electrical Resistivity | 0.0000510 ohm-cm |
|
Magnetic Properties | Original Value | Comments |
---|
Core Loss | 0.00183 W/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00189 W/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00242 W/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00249 W/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00702 W/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.00707 W/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.00928 W/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.00935 W/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0152 W/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0153 W/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0202 W/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0202 W/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0264 W/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0265 W/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0346 W/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0347 W/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0400 W/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0402 W/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0528 W/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0531 W/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0564 W/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0568 W/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0742 W/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.0748 W/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.0753 W/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.0761 W/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.0968 W/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.0981 W/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.0990 W/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.100 W/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.121 W/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.123 W/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.127 W/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.129 W/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.148 W/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.151 W/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.159 W/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.162 W/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.179 W/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.182 W/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.195 W/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.198 W/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.214 W/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.217 W/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.236 W/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.239 W/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.253 W/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.255 W/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.281 W/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.285 W/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.298 W/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.300 W/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.333 W/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.336 W/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.351 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.353 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.354 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| <= 0.390 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.391 W/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.395 W/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.418 W/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.421 W/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.460 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.462 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.463 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| <= 0.510 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.514 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.518 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.520 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.546 W/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.550 W/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| <= 0.560 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.658 W/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 0.666 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 0.670 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 0.673 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 0.680 W/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| <= 0.740 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 0.770 W/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 0.845 W/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 0.845 W/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 0.872 W/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 0.990 W/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
| 1.09 W/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
|
Descriptive Properties |
---|
Magnetostriction 10^8 | -116 |
| -93 |
Minimum Lamination Factor (%) | 95 |
Minimum Peak Permeability at 10 Oe | 1780 |
Typical Lamination Factor (%) | 96.9 |
Typical Peak Permeability at 10 Oe | 1845 |