MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AK Steel CARLITE® M-4 Grain Oriented Electrical Steel (Extended Electro-Magnetic Data)
Categories: Metal; Electronic/Magnetic Alloy

Material Notes: Oriented Electrical Steels are iron-silicon alloys that were developed to provide the low core loss and high permeability required for efficient and economical electrical transformers. First produced commercially by AK Steel, these magnetic materials exhibit their superior magnetic properties in the rolling direction. This directionality occurs because the steels are specially processed to create a very high proportion of grains within the steel which have similarly oriented atomic crystalline structures relative to the rolling direction.

In iron-silicon alloys, this atomic structure is cubic and the crystals are most easily magnetized in a direction parallel to the cube edges. By a combination of precise steel composition, rigidly controlled cold rolling and annealing procedures, the crystals of these oriented electrical steels are aligned with their cube edges nearly parallel to the direction in which the steel is rolled. Consequently, they provide superior permeability and lower core loss when magnetized in this direction.

AK Steel’s CARLITE grain Oriented Electrical Steels (GOES) products are supplied with CARLITE 3 insulative coating, an inorganic coating equivalent to ASTM A976 C-5. CARLITE 3 insulation is ideal for materials that will be used in the form of sheared laminations for power transformers and other apparatus with high volts per turn. In addition to supplying all the benefits of C-5 insulation, CARLITE 3 provides other important advantages which include:

  • Potential for reduced transformer building factor from added resistance to elastic strain damage
  • Potential for reduction of magnetostriction related transformer noise
  • High stacking factor
  • Easy assembly due to smoothness of coating (low coefficient of friction)

Information provided by AK Steel

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.65 g/cc0.276 lb/in³
Thickness 279 microns11.0 milNominal
 
Mechanical PropertiesMetricEnglishComments
Hardness, Knoop 167167
Hardness, Rockwell B 8181
Tensile Strength, Ultimate 352 MPa51000 psiIn rolling direction
Tensile Strength, Yield 331 MPa48000 psiIn rolling direction
Elongation at Break 9.0 %9.0 %in 2"
Modulus of Elasticity 122 GPa17700 ksiIn rolling direction
 143 GPa20700 ksiat 20° to rolling direction
 200 GPa29000 ksiat 55° to rolling direction
 236 GPa34200 ksiat 90° to rolling direction
 258 GPa37400 ksiat 45° to rolling direction
 
Electrical PropertiesMetricEnglishComments
Exciting Power (RMS)  0.00268 RMS AT/cm
@Magnetic Field 0.100 T,
Frequency 50 Hz
0.00424 RMS VA/lb
@Magnetic Field 0.100 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.00299 RMS AT/cm
@Magnetic Field 0.100 T,
Frequency 50 Hz
0.00472 RMS VA/lb
@Magnetic Field 0.100 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.00332 RMS AT/cm
@Magnetic Field 0.100 T,
Frequency 60 Hz
0.00524 RMS VA/lb
@Magnetic Field 0.100 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.00369 RMS AT/cm
@Magnetic Field 0.100 T,
Frequency 60 Hz
0.00583 RMS VA/lb
@Magnetic Field 0.100 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.00892 RMS AT/cm
@Magnetic Field 0.200 T,
Frequency 50 Hz
0.0141 RMS VA/lb
@Magnetic Field 0.200 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.00974 RMS AT/cm
@Magnetic Field 0.200 T,
Frequency 50 Hz
0.0154 RMS VA/lb
@Magnetic Field 0.200 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.0111 RMS AT/cm
@Magnetic Field 0.200 T,
Frequency 60 Hz
0.0176 RMS VA/lb
@Magnetic Field 0.200 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.0121 RMS AT/cm
@Magnetic Field 0.200 T,
Frequency 60 Hz
0.0192 RMS VA/lb
@Magnetic Field 0.200 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.0179 RMS AT/cm
@Magnetic Field 0.300 T,
Frequency 50 Hz
0.0283 RMS VA/lb
@Magnetic Field 0.300 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.0193 RMS AT/cm
@Magnetic Field 0.300 T,
Frequency 50 Hz
0.0305 RMS VA/lb
@Magnetic Field 0.300 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.0224 RMS AT/cm
@Magnetic Field 0.300 T,
Frequency 60 Hz
0.0354 RMS VA/lb
@Magnetic Field 0.300 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.0241 RMS AT/cm
@Magnetic Field 0.300 T,
Frequency 60 Hz
0.0381 RMS VA/lb
@Magnetic Field 0.300 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.0289 RMS AT/cm
@Magnetic Field 0.400 T,
Frequency 50 Hz
0.0457 RMS VA/lb
@Magnetic Field 0.400 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.0309 RMS AT/cm
@Magnetic Field 0.400 T,
Frequency 50 Hz
0.0488 RMS VA/lb
@Magnetic Field 0.400 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.0363 RMS AT/cm
@Magnetic Field 0.400 T,
Frequency 60 Hz
0.0574 RMS VA/lb
@Magnetic Field 0.400 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.0388 RMS AT/cm
@Magnetic Field 0.400 T,
Frequency 60 Hz
0.0613 RMS VA/lb
@Magnetic Field 0.400 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.0417 RMS AT/cm
@Magnetic Field 0.500 T,
Frequency 50 Hz
0.0659 RMS VA/lb
@Magnetic Field 0.500 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.0442 RMS AT/cm
@Magnetic Field 0.500 T,
Frequency 50 Hz
0.0699 RMS VA/lb
@Magnetic Field 0.500 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.0526 RMS AT/cm
@Magnetic Field 0.500 T,
Frequency 60 Hz
0.0831 RMS VA/lb
@Magnetic Field 0.500 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.0557 RMS AT/cm
@Magnetic Field 0.500 T,
Frequency 60 Hz
0.0881 RMS VA/lb
@Magnetic Field 0.500 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.0561 RMS AT/cm
@Magnetic Field 0.600 T,
Frequency 50 Hz
0.0887 RMS VA/lb
@Magnetic Field 0.600 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.0593 RMS AT/cm
@Magnetic Field 0.600 T,
Frequency 50 Hz
0.0937 RMS VA/lb
@Magnetic Field 0.600 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.0709 RMS AT/cm
@Magnetic Field 0.600 T,
Frequency 60 Hz
0.112 RMS VA/lb
@Magnetic Field 0.600 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.0721 RMS AT/cm
@Magnetic Field 0.700 T,
Frequency 50 Hz
0.114 RMS VA/lb
@Magnetic Field 0.700 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.0747 RMS AT/cm
@Magnetic Field 0.600 T,
Frequency 60 Hz
0.118 RMS VA/lb
@Magnetic Field 0.600 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.0759 RMS AT/cm
@Magnetic Field 0.700 T,
Frequency 50 Hz
0.120 RMS VA/lb
@Magnetic Field 0.700 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.0898 RMS AT/cm
@Magnetic Field 0.800 T,
Frequency 50 Hz
0.142 RMS VA/lb
@Magnetic Field 0.800 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.0917 RMS AT/cm
@Magnetic Field 0.700 T,
Frequency 60 Hz
0.145 RMS VA/lb
@Magnetic Field 0.700 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.0943 RMS AT/cm
@Magnetic Field 0.800 T,
Frequency 50 Hz
0.149 RMS VA/lb
@Magnetic Field 0.800 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.0962 RMS AT/cm
@Magnetic Field 0.700 T,
Frequency 60 Hz
0.152 RMS VA/lb
@Magnetic Field 0.700 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.109 RMS AT/cm
@Magnetic Field 0.900 T,
Frequency 50 Hz
0.173 RMS VA/lb
@Magnetic Field 0.900 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.115 RMS AT/cm
@Magnetic Field 0.800 T,
Frequency 60 Hz
0.181 RMS VA/lb
@Magnetic Field 0.800 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.115 RMS AT/cm
@Magnetic Field 0.900 T,
Frequency 50 Hz
0.181 RMS VA/lb
@Magnetic Field 0.900 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.120 RMS AT/cm
@Magnetic Field 0.800 T,
Frequency 60 Hz
0.189 RMS VA/lb
@Magnetic Field 0.800 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.132 RMS AT/cm
@Magnetic Field 1.00 T,
Frequency 50 Hz
0.208 RMS VA/lb
@Magnetic Field 1.00 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.138 RMS AT/cm
@Magnetic Field 1.00 T,
Frequency 50 Hz
0.218 RMS VA/lb
@Magnetic Field 1.00 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.140 RMS AT/cm
@Magnetic Field 0.900 T,
Frequency 60 Hz
0.221 RMS VA/lb
@Magnetic Field 0.900 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.146 RMS AT/cm
@Magnetic Field 0.900 T,
Frequency 60 Hz
0.231 RMS VA/lb
@Magnetic Field 0.900 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.157 RMS AT/cm
@Magnetic Field 1.10 T,
Frequency 50 Hz
0.248 RMS VA/lb
@Magnetic Field 1.10 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.163 RMS AT/cm
@Magnetic Field 1.10 T,
Frequency 50 Hz
0.258 RMS VA/lb
@Magnetic Field 1.10 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.168 RMS AT/cm
@Magnetic Field 1.00 T,
Frequency 60 Hz
0.265 RMS VA/lb
@Magnetic Field 1.00 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.175 RMS AT/cm
@Magnetic Field 1.00 T,
Frequency 60 Hz
0.277 RMS VA/lb
@Magnetic Field 1.00 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.186 RMS AT/cm
@Magnetic Field 1.20 T,
Frequency 50 Hz
0.294 RMS VA/lb
@Magnetic Field 1.20 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.194 RMS AT/cm
@Magnetic Field 1.20 T,
Frequency 50 Hz
0.306 RMS VA/lb
@Magnetic Field 1.20 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.200 RMS AT/cm
@Magnetic Field 1.10 T,
Frequency 60 Hz
0.316 RMS VA/lb
@Magnetic Field 1.10 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.208 RMS AT/cm
@Magnetic Field 1.10 T,
Frequency 60 Hz
0.329 RMS VA/lb
@Magnetic Field 1.10 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.222 RMS AT/cm
@Magnetic Field 1.30 T,
Frequency 50 Hz
0.351 RMS VA/lb
@Magnetic Field 1.30 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.231 RMS AT/cm
@Magnetic Field 1.30 T,
Frequency 50 Hz
0.365 RMS VA/lb
@Magnetic Field 1.30 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.237 RMS AT/cm
@Magnetic Field 1.20 T,
Frequency 60 Hz
0.374 RMS VA/lb
@Magnetic Field 1.20 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.246 RMS AT/cm
@Magnetic Field 1.20 T,
Frequency 60 Hz
0.389 RMS VA/lb
@Magnetic Field 1.20 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.268 RMS AT/cm
@Magnetic Field 1.40 T,
Frequency 50 Hz
0.424 RMS VA/lb
@Magnetic Field 1.40 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.276 RMS AT/cm
@Magnetic Field 1.40 T,
Frequency 50 Hz
0.437 RMS VA/lb
@Magnetic Field 1.40 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.282 RMS AT/cm
@Magnetic Field 1.30 T,
Frequency 60 Hz
0.445 RMS VA/lb
@Magnetic Field 1.30 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.293 RMS AT/cm
@Magnetic Field 1.30 T,
Frequency 60 Hz
0.463 RMS VA/lb
@Magnetic Field 1.30 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.337 RMS AT/cm
@Magnetic Field 1.50 T,
Frequency 50 Hz
0.533 RMS VA/lb
@Magnetic Field 1.50 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.340 RMS AT/cm
@Magnetic Field 1.40 T,
Frequency 60 Hz
0.537 RMS VA/lb
@Magnetic Field 1.40 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.349 RMS AT/cm
@Magnetic Field 1.50 T,
Frequency 50 Hz
0.552 RMS VA/lb
@Magnetic Field 1.50 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.423 RMS AT/cm
@Magnetic Field 1.50 T,
Frequency 60 Hz
0.669 RMS VA/lb
@Magnetic Field 1.50 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.439 RMS AT/cm
@Magnetic Field 1.50 T,
Frequency 60 Hz
0.694 RMS VA/lb
@Magnetic Field 1.50 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.450 RMS AT/cm
@Magnetic Field 1.60 T,
Frequency 50 Hz
0.711 RMS VA/lb
@Magnetic Field 1.60 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.459 RMS AT/cm
@Magnetic Field 1.60 T,
Frequency 50 Hz
0.726 RMS VA/lb
@Magnetic Field 1.60 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.553 RMS AT/cm
@Magnetic Field 1.40 T,
Frequency 60 Hz
0.874 RMS VA/lb
@Magnetic Field 1.40 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.559 RMS AT/cm
@Magnetic Field 1.60 T,
Frequency 60 Hz
0.883 RMS VA/lb
@Magnetic Field 1.60 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.570 RMS AT/cm
@Magnetic Field 1.60 T,
Frequency 60 Hz
0.901 RMS VA/lb
@Magnetic Field 1.60 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.785 RMS AT/cm
@Magnetic Field 1.70 T,
Frequency 50 Hz
1.24 RMS VA/lb
@Magnetic Field 1.70 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.791 RMS AT/cm
@Magnetic Field 1.70 T,
Frequency 50 Hz
1.25 RMS VA/lb
@Magnetic Field 1.70 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.962 RMS AT/cm
@Magnetic Field 1.70 T,
Frequency 60 Hz
1.52 RMS VA/lb
@Magnetic Field 1.70 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.968 RMS AT/cm
@Magnetic Field 1.70 T,
Frequency 60 Hz
1.53 RMS VA/lb
@Magnetic Field 1.70 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 2.21 RMS AT/cm
@Magnetic Field 1.80 T,
Frequency 50 Hz
3.50 RMS VA/lb
@Magnetic Field 1.80 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 2.35 RMS AT/cm
@Magnetic Field 1.80 T,
Frequency 50 Hz
3.72 RMS VA/lb
@Magnetic Field 1.80 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 2.69 RMS AT/cm
@Magnetic Field 1.80 T,
Frequency 60 Hz
4.25 RMS VA/lb
@Magnetic Field 1.80 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 2.86 RMS AT/cm
@Magnetic Field 1.80 T,
Frequency 60 Hz
4.52 RMS VA/lb
@Magnetic Field 1.80 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 7.85 RMS AT/cm
@Magnetic Field 1.90 T,
Frequency 50 Hz
12.4 RMS VA/lb
@Magnetic Field 1.90 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 9.55 RMS AT/cm
@Magnetic Field 1.90 T,
Frequency 60 Hz
15.1 RMS VA/lb
@Magnetic Field 1.90 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 10.4 RMS AT/cm
@Magnetic Field 1.90 T,
Frequency 50 Hz
16.4 RMS VA/lb
@Magnetic Field 1.90 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 12.7 RMS AT/cm
@Magnetic Field 1.90 T,
Frequency 60 Hz
20.0 RMS VA/lb
@Magnetic Field 1.90 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
Electrical Resistivity 0.0000510 ohm-cm0.0000510 ohm-cm
 
Magnetic PropertiesMetricEnglishComments
Core Loss  0.00403 W/kg
@Magnetic Field 0.100 T,
Frequency 50 Hz
0.00183 W/lb
@Magnetic Field 0.100 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.00417 W/kg
@Magnetic Field 0.100 T,
Frequency 50 Hz
0.00189 W/lb
@Magnetic Field 0.100 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.00534 W/kg
@Magnetic Field 0.100 T,
Frequency 60 Hz
0.00242 W/lb
@Magnetic Field 0.100 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.00549 W/kg
@Magnetic Field 0.100 T,
Frequency 60 Hz
0.00249 W/lb
@Magnetic Field 0.100 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.0155 W/kg
@Magnetic Field 0.200 T,
Frequency 50 Hz
0.00702 W/lb
@Magnetic Field 0.200 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.0156 W/kg
@Magnetic Field 0.200 T,
Frequency 50 Hz
0.00707 W/lb
@Magnetic Field 0.200 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.0205 W/kg
@Magnetic Field 0.200 T,
Frequency 60 Hz
0.00928 W/lb
@Magnetic Field 0.200 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.0206 W/kg
@Magnetic Field 0.200 T,
Frequency 60 Hz
0.00935 W/lb
@Magnetic Field 0.200 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.0335 W/kg
@Magnetic Field 0.300 T,
Frequency 50 Hz
0.0152 W/lb
@Magnetic Field 0.300 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.0337 W/kg
@Magnetic Field 0.300 T,
Frequency 50 Hz
0.0153 W/lb
@Magnetic Field 0.300 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.0445 W/kg
@Magnetic Field 0.300 T,
Frequency 60 Hz
0.0202 W/lb
@Magnetic Field 0.300 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.0445 W/kg
@Magnetic Field 0.300 T,
Frequency 60 Hz
0.0202 W/lb
@Magnetic Field 0.300 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.0582 W/kg
@Magnetic Field 0.400 T,
Frequency 50 Hz
0.0264 W/lb
@Magnetic Field 0.400 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.0584 W/kg
@Magnetic Field 0.400 T,
Frequency 50 Hz
0.0265 W/lb
@Magnetic Field 0.400 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.0763 W/kg
@Magnetic Field 0.400 T,
Frequency 60 Hz
0.0346 W/lb
@Magnetic Field 0.400 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.0765 W/kg
@Magnetic Field 0.400 T,
Frequency 60 Hz
0.0347 W/lb
@Magnetic Field 0.400 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.0882 W/kg
@Magnetic Field 0.500 T,
Frequency 50 Hz
0.0400 W/lb
@Magnetic Field 0.500 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.0886 W/kg
@Magnetic Field 0.500 T,
Frequency 50 Hz
0.0402 W/lb
@Magnetic Field 0.500 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.116 W/kg
@Magnetic Field 0.500 T,
Frequency 60 Hz
0.0528 W/lb
@Magnetic Field 0.500 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.117 W/kg
@Magnetic Field 0.500 T,
Frequency 60 Hz
0.0531 W/lb
@Magnetic Field 0.500 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.124 W/kg
@Magnetic Field 0.600 T,
Frequency 50 Hz
0.0564 W/lb
@Magnetic Field 0.600 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.125 W/kg
@Magnetic Field 0.600 T,
Frequency 50 Hz
0.0568 W/lb
@Magnetic Field 0.600 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.164 W/kg
@Magnetic Field 0.600 T,
Frequency 60 Hz
0.0742 W/lb
@Magnetic Field 0.600 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.165 W/kg
@Magnetic Field 0.600 T,
Frequency 60 Hz
0.0748 W/lb
@Magnetic Field 0.600 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.166 W/kg
@Magnetic Field 0.700 T,
Frequency 50 Hz
0.0753 W/lb
@Magnetic Field 0.700 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.168 W/kg
@Magnetic Field 0.700 T,
Frequency 50 Hz
0.0761 W/lb
@Magnetic Field 0.700 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.213 W/kg
@Magnetic Field 0.800 T,
Frequency 50 Hz
0.0968 W/lb
@Magnetic Field 0.800 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.216 W/kg
@Magnetic Field 0.800 T,
Frequency 50 Hz
0.0981 W/lb
@Magnetic Field 0.800 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.218 W/kg
@Magnetic Field 0.700 T,
Frequency 60 Hz
0.0990 W/lb
@Magnetic Field 0.700 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.220 W/kg
@Magnetic Field 0.700 T,
Frequency 60 Hz
0.100 W/lb
@Magnetic Field 0.700 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.267 W/kg
@Magnetic Field 0.900 T,
Frequency 50 Hz
0.121 W/lb
@Magnetic Field 0.900 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.271 W/kg
@Magnetic Field 0.900 T,
Frequency 50 Hz
0.123 W/lb
@Magnetic Field 0.900 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.280 W/kg
@Magnetic Field 0.800 T,
Frequency 60 Hz
0.127 W/lb
@Magnetic Field 0.800 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.284 W/kg
@Magnetic Field 0.800 T,
Frequency 60 Hz
0.129 W/lb
@Magnetic Field 0.800 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.326 W/kg
@Magnetic Field 1.00 T,
Frequency 50 Hz
0.148 W/lb
@Magnetic Field 1.00 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.333 W/kg
@Magnetic Field 1.00 T,
Frequency 50 Hz
0.151 W/lb
@Magnetic Field 1.00 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.351 W/kg
@Magnetic Field 0.900 T,
Frequency 60 Hz
0.159 W/lb
@Magnetic Field 0.900 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.357 W/kg
@Magnetic Field 0.900 T,
Frequency 60 Hz
0.162 W/lb
@Magnetic Field 0.900 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.395 W/kg
@Magnetic Field 1.10 T,
Frequency 50 Hz
0.179 W/lb
@Magnetic Field 1.10 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.401 W/kg
@Magnetic Field 1.10 T,
Frequency 50 Hz
0.182 W/lb
@Magnetic Field 1.10 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.430 W/kg
@Magnetic Field 1.00 T,
Frequency 60 Hz
0.195 W/lb
@Magnetic Field 1.00 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.437 W/kg
@Magnetic Field 1.00 T,
Frequency 60 Hz
0.198 W/lb
@Magnetic Field 1.00 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.472 W/kg
@Magnetic Field 1.20 T,
Frequency 50 Hz
0.214 W/lb
@Magnetic Field 1.20 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.478 W/kg
@Magnetic Field 1.20 T,
Frequency 50 Hz
0.217 W/lb
@Magnetic Field 1.20 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.520 W/kg
@Magnetic Field 1.10 T,
Frequency 60 Hz
0.236 W/lb
@Magnetic Field 1.10 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.527 W/kg
@Magnetic Field 1.10 T,
Frequency 60 Hz
0.239 W/lb
@Magnetic Field 1.10 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.558 W/kg
@Magnetic Field 1.30 T,
Frequency 50 Hz
0.253 W/lb
@Magnetic Field 1.30 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.562 W/kg
@Magnetic Field 1.30 T,
Frequency 50 Hz
0.255 W/lb
@Magnetic Field 1.30 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.619 W/kg
@Magnetic Field 1.20 T,
Frequency 60 Hz
0.281 W/lb
@Magnetic Field 1.20 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.628 W/kg
@Magnetic Field 1.20 T,
Frequency 60 Hz
0.285 W/lb
@Magnetic Field 1.20 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.657 W/kg
@Magnetic Field 1.40 T,
Frequency 50 Hz
0.298 W/lb
@Magnetic Field 1.40 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.661 W/kg
@Magnetic Field 1.40 T,
Frequency 50 Hz
0.300 W/lb
@Magnetic Field 1.40 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.734 W/kg
@Magnetic Field 1.30 T,
Frequency 60 Hz
0.333 W/lb
@Magnetic Field 1.30 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.741 W/kg
@Magnetic Field 1.30 T,
Frequency 60 Hz
0.336 W/lb
@Magnetic Field 1.30 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.774 W/kg
@Magnetic Field 1.50 T,
Frequency 50 Hz
0.351 W/lb
@Magnetic Field 1.50 T,
Frequency 50 Hz
Typical
 0.778 W/kg
@Magnetic Field 1.50 T,
Frequency 50 Hz
0.353 W/lb
@Magnetic Field 1.50 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.780 W/kg
@Magnetic Field 1.50 T,
Frequency 50 Hz
0.354 W/lb
@Magnetic Field 1.50 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 <= 0.860 W/kg
@Magnetic Field 1.50 T,
Frequency 50 Hz
<= 0.390 W/lb
@Magnetic Field 1.50 T,
Frequency 50 Hz
 0.862 W/kg
@Magnetic Field 1.40 T,
Frequency 60 Hz
0.391 W/lb
@Magnetic Field 1.40 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 0.871 W/kg
@Magnetic Field 1.40 T,
Frequency 60 Hz
0.395 W/lb
@Magnetic Field 1.40 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 0.922 W/kg
@Magnetic Field 1.60 T,
Frequency 50 Hz
0.418 W/lb
@Magnetic Field 1.60 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 0.928 W/kg
@Magnetic Field 1.60 T,
Frequency 50 Hz
0.421 W/lb
@Magnetic Field 1.60 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 1.01 W/kg
@Magnetic Field 1.50 T,
Frequency 60 Hz
0.460 W/lb
@Magnetic Field 1.50 T,
Frequency 60 Hz
Typical
 1.02 W/kg
@Magnetic Field 1.50 T,
Frequency 60 Hz
0.462 W/lb
@Magnetic Field 1.50 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 1.02 W/kg
@Magnetic Field 1.50 T,
Frequency 60 Hz
0.463 W/lb
@Magnetic Field 1.50 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 <= 1.12 W/kg
@Magnetic Field 1.50 T,
Frequency 60 Hz
<= 0.510 W/lb
@Magnetic Field 1.50 T,
Frequency 60 Hz
 1.13 W/kg
@Magnetic Field 1.70 T,
Frequency 50 Hz
0.514 W/lb
@Magnetic Field 1.70 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 1.14 W/kg
@Magnetic Field 1.70 T,
Frequency 50 Hz
0.518 W/lb
@Magnetic Field 1.70 T,
Frequency 50 Hz
Typical
 1.15 W/kg
@Magnetic Field 1.70 T,
Frequency 50 Hz
0.520 W/lb
@Magnetic Field 1.70 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 1.20 W/kg
@Magnetic Field 1.60 T,
Frequency 60 Hz
0.546 W/lb
@Magnetic Field 1.60 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 1.21 W/kg
@Magnetic Field 1.60 T,
Frequency 60 Hz
0.550 W/lb
@Magnetic Field 1.60 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 <= 1.23 W/kg
@Magnetic Field 1.70 T,
Frequency 50 Hz
<= 0.560 W/lb
@Magnetic Field 1.70 T,
Frequency 50 Hz
 1.45 W/kg
@Magnetic Field 1.80 T,
Frequency 50 Hz
0.658 W/lb
@Magnetic Field 1.80 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 1.47 W/kg
@Magnetic Field 1.70 T,
Frequency 60 Hz
0.666 W/lb
@Magnetic Field 1.70 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 1.48 W/kg
@Magnetic Field 1.70 T,
Frequency 60 Hz
0.670 W/lb
@Magnetic Field 1.70 T,
Frequency 60 Hz
Typical
 1.48 W/kg
@Magnetic Field 1.70 T,
Frequency 60 Hz
0.673 W/lb
@Magnetic Field 1.70 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 1.50 W/kg
@Magnetic Field 1.80 T,
Frequency 50 Hz
0.680 W/lb
@Magnetic Field 1.80 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 <= 1.63 W/kg
@Magnetic Field 1.70 T,
Frequency 60 Hz
<= 0.740 W/lb
@Magnetic Field 1.70 T,
Frequency 60 Hz
 1.70 W/kg
@Magnetic Field 1.90 T,
Frequency 50 Hz
0.770 W/lb
@Magnetic Field 1.90 T,
Frequency 50 Hz
Sheet, 0.011"; ASTM A804
 1.86 W/kg
@Magnetic Field 1.80 T,
Frequency 60 Hz
0.845 W/lb
@Magnetic Field 1.80 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 1.86 W/kg
@Magnetic Field 1.90 T,
Frequency 50 Hz
0.845 W/lb
@Magnetic Field 1.90 T,
Frequency 50 Hz
Epstein Specimen, 0.011"; ASTM A343
 1.92 W/kg
@Magnetic Field 1.80 T,
Frequency 60 Hz
0.872 W/lb
@Magnetic Field 1.80 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 2.18 W/kg
@Magnetic Field 1.90 T,
Frequency 60 Hz
0.990 W/lb
@Magnetic Field 1.90 T,
Frequency 60 Hz
Sheet, 0.011"; ASTM A804
 2.40 W/kg
@Magnetic Field 1.90 T,
Frequency 60 Hz
1.09 W/lb
@Magnetic Field 1.90 T,
Frequency 60 Hz
Epstein Specimen, 0.011"; ASTM A343
 
Descriptive Properties
Magnetostriction 10^8-116At 60Hz, 1.7T (Thickness 0.011")
 -93At 60Hz, 1.5T (Thickness 0.011")
Minimum Lamination Factor (%)95
Minimum Peak Permeability at 10 Oe1780
Typical Lamination Factor (%)96.9
Typical Peak Permeability at 10 Oe1845

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AK Steel CARLITE® M-6 Grain Oriented Electrical Steel (Extended Electro-Magnetic Data)
AK Steel CARLITE® M-3 Grain Oriented Electrical Steel (Extended Electro-Magnetic Data)
AK Steel CARLITE® M-3 Grain Oriented Electrical Steel
AK Steel CARLITE® M-5 Grain Oriented Electrical Steel (Extended Electro-Magnetic Data)
AK Steel TRAN-COR® H-1 CARLITE® Grain Oriented Electrical Steel

NAKS151a / 171254

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.