MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AK Steel TRAN-COR® H-1 CARLITE® DR® Grain Oriented Electrical Steel
Categories: Metal; Electronic/Magnetic Alloy; Ferrous Metal

Material Notes: TRAN-COR H CARLITE® high permeability electrical steels offer an outstanding degree of grain orientation, This combination of higher permeability with low residual stress offers the potential for lower core losses and less noisy transformer core structures, particularly at higher operating inductions, when compared to conventional grain oriented electrical steels. The core loss characteristics are further enhanced in the TRAN-COR H CARLITE DR® (Domain Refined) products where laser scribing is employed. In this process, a precisely focused laser beam is rapidly scanned across the steel surface. The micro-strain imparted into the material forces the pre-existing magnetic domains to subdivide. The finer domain structure reduces the distance that the domain walls must move during AC magnetization, thereby reducing eddy current losses. The result is far lower core loss than possible with conventional grain oriented electrical steels of comparable thickness. TRAN-COR H CARLITE products are suitable for all types of transformers while TRAN-COR H DR products are suitable for those types of transformers where a stress relief annealing treatment of the magnetic core is not used. Stress relief annealing will result in the eradication of the effect provided by the laser treatment and will result in a significant increase in core loss.

Information provided by AK Steel.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.65 g/cc
Thickness 240 - 280 microns
 270 micronsNominal
 
Mechanical PropertiesOriginal ValueComments
Knoop Microhardness 173
Hardness, Rockwell B 83
Tensile Strength, Ultimate 359 MPaIn rolling direction
Tensile Strength, Yield 345 MPaIn rolling direction
Elongation at Break 11 %In 2", rolling direction
Modulus of Elasticity 113.8 GPaIn rolling direction
 138 GPaAt 20° to rolling direction
 203 GPaAt 90° to rolling direction
 241 GPaAt 45° to rolling direction
 276 GPaAt 55° to rolling direction
 
Electrical PropertiesOriginal ValueComments
Exciting Power (RMS) 0.00250 RMS VA/lb
@Magnetic Field 0.100 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.00310 RMS VA/lb
@Magnetic Field 0.100 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.00870 RMS VA/lb
@Magnetic Field 0.200 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.0111 RMS VA/lb
@Magnetic Field 0.200 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.0184 RMS VA/lb
@Magnetic Field 0.300 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.0235 RMS VA/lb
@Magnetic Field 0.300 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.0310 RMS VA/lb
@Magnetic Field 0.400 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.0397 RMS VA/lb
@Magnetic Field 0.400 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.0461 RMS VA/lb
@Magnetic Field 0.500 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.0594 RMS VA/lb
@Magnetic Field 0.500 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.0637 RMS VA/lb
@Magnetic Field 0.600 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.0822 RMS VA/lb
@Magnetic Field 0.600 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.0839 RMS VA/lb
@Magnetic Field 0.700 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.1068 RMS VA/lb
@Magnetic Field 0.800 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.1082 RMS VA/lb
@Magnetic Field 0.700 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.1327 RMS VA/lb
@Magnetic Field 0.900 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.1377 RMS VA/lb
@Magnetic Field 0.800 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.1632 RMS VA/lb
@Magnetic Field 1.00 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.1714 RMS VA/lb
@Magnetic Field 0.900 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.1995 RMS VA/lb
@Magnetic Field 1.10 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.2105 RMS VA/lb
@Magnetic Field 1.00 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.2427 RMS VA/lb
@Magnetic Field 1.20 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.2568 RMS VA/lb
@Magnetic Field 1.10 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.2955 RMS VA/lb
@Magnetic Field 1.30 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.3114 RMS VA/lb
@Magnetic Field 1.20 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.3586 RMS VA/lb
@Magnetic Field 1.40 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.3768 RMS VA/lb
@Magnetic Field 1.30 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.4336 RMS VA/lb
@Magnetic Field 1.50 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.4541 RMS VA/lb
@Magnetic Field 1.40 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.5282 RMS VA/lb
@Magnetic Field 1.60 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.5455 RMS VA/lb
@Magnetic Field 1.50 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.6605 RMS VA/lb
@Magnetic Field 1.60 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.6936 RMS VA/lb
@Magnetic Field 1.70 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.8577 RMS VA/lb
@Magnetic Field 1.70 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 1.20 RMS VA/lb
@Magnetic Field 1.80 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 1.4591 RMS VA/lb
@Magnetic Field 1.80 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 4.1682 RMS VA/lb
@Magnetic Field 1.90 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 5.0682 RMS VA/lb
@Magnetic Field 1.90 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
Electrical Resistivity 0.0000500 ohm-cm
 
Magnetic PropertiesOriginal ValueComments
Core Loss 0.00328 W/kg
@Magnetic Field 0.100 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.00441 W/kg
@Magnetic Field 0.100 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.01246 W/kg
@Magnetic Field 0.200 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.0168 W/kg
@Magnetic Field 0.200 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.0274 W/kg
@Magnetic Field 0.300 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.0370 W/kg
@Magnetic Field 0.300 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.0479 W/kg
@Magnetic Field 0.400 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.0647 W/kg
@Magnetic Field 0.400 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.0738 W/kg
@Magnetic Field 0.500 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.0996 W/kg
@Magnetic Field 0.500 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.105 W/kg
@Magnetic Field 0.600 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.1413 W/kg
@Magnetic Field 0.600 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.1415 W/kg
@Magnetic Field 0.700 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.1837 W/kg
@Magnetic Field 0.800 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.190 W/kg
@Magnetic Field 0.700 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.231 W/kg
@Magnetic Field 0.900 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.246 W/kg
@Magnetic Field 0.800 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.284 W/kg
@Magnetic Field 1.00 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.309 W/kg
@Magnetic Field 0.900 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.344 W/kg
@Magnetic Field 1.10 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.380 W/kg
@Magnetic Field 1.00 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.410 W/kg
@Magnetic Field 1.20 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.459 W/kg
@Magnetic Field 1.10 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.483 W/kg
@Magnetic Field 1.30 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.547 W/kg
@Magnetic Field 1.20 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.562 W/kg
@Magnetic Field 1.40 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.644 W/kg
@Magnetic Field 1.30 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.649 W/kg
@Magnetic Field 1.50 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.650 W/kg
@Magnetic Field 1.50 T,
Frequency 50 Hz
Typical
 0.748 W/kg
@Magnetic Field 1.60 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.749 W/kg
@Magnetic Field 1.40 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.860 W/kg
@Magnetic Field 1.50 T,
Frequency 60 Hz
Typical
 0.865 W/kg
@Magnetic Field 1.50 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 0.870 W/kg
@Magnetic Field 1.70 T,
Frequency 50 Hz
Typical
 0.872 W/kg
@Magnetic Field 1.70 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 0.900 W/kg
@Magnetic Field 1.70 T,
Frequency 50 Hz
Maximum
 0.994 W/kg
@Magnetic Field 1.60 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 1.067 W/kg
@Magnetic Field 1.80 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 1.154 W/kg
@Magnetic Field 1.70 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 1.16 W/kg
@Magnetic Field 1.70 T,
Frequency 60 Hz
Typical
 1.20 W/kg
@Magnetic Field 1.70 T,
Frequency 60 Hz
Maximum
 1.405 W/kg
@Magnetic Field 1.80 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 1.44 W/kg
@Magnetic Field 1.90 T,
Frequency 50 Hz
ASTM A804, 0.27 mm
 1.876 W/kg
@Magnetic Field 1.90 T,
Frequency 60 Hz
ASTM A804, 0.27 mm
 
Descriptive Properties
Approximate Equivalent International GradeM090-27P5
Magnetostriction 10^8-22ASTM A876, 1.4T, 60Hz, 0.27 mm
 -25ASTM A876, 1.5T, 60Hz, 0.27 mm
 -26ASTM A876, 1.6T, 60Hz, 0.27 mm
 -28ASTM A876, 1.7T, 60Hz, 0.27 mm
Maximum Induction at 800 A/m (T)1.88
Minimum Lamination Factor (%)95
Typical Induction at 800 A/m (T)1.918
Typical Lamination Factor (%)97

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AK Steel DI-MAX® HF-10 Nonoriented Electrical Steel (Extended Electrical/Magnetic Data)
AK Steel TRAN-COR® H-0 CARLITE® DR® Grain Oriented Electrical Steel
AK Steel TRAN-COR® H-1 CARLITE® Grain Oriented Electrical Steel
AK Steel DI-MAX® M-15 Nonoriented Electrical Steel
AK Steel DI-MAX® HF-10 Nonoriented Electrical Steel

NAKS167 / 140763

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.