Physical Properties | Metric | English | Comments |
---|
Density | 7.65 g/cc | 0.276 lb/in³ |
Thickness | 200 - 240 microns | 7.87 - 9.45 mil |
| 230 microns | 9.06 mil |
|
Mechanical Properties | Metric | English | Comments |
---|
Knoop Microhardness | 173 | 173 |
Hardness, Rockwell B | 83 | 83 |
Tensile Strength, Ultimate | 359 MPa | 52100 psi |
Tensile Strength, Yield | 345 MPa | 50000 psi |
Elongation at Break | 11 % | 11 % |
Modulus of Elasticity | 113.8 GPa | 16510 ksi |
| 138 GPa | 20000 ksi |
| 203 GPa | 29400 ksi |
| 241 GPa | 35000 ksi |
| 276 GPa | 40000 ksi |
|
Electrical Properties | Metric | English | Comments |
---|
Exciting Power (RMS) | 0.00165 RMS AT/cm @Magnetic Field 0.100 T, Frequency 50 Hz | 0.00260 RMS VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00209 RMS AT/cm @Magnetic Field 0.100 T, Frequency 60 Hz | 0.00330 RMS VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00576 RMS AT/cm @Magnetic Field 0.200 T, Frequency 50 Hz | 0.00910 RMS VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.00721 RMS AT/cm @Magnetic Field 0.200 T, Frequency 60 Hz | 0.0114 RMS VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0120 RMS AT/cm @Magnetic Field 0.300 T, Frequency 50 Hz | 0.0190 RMS VA/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0151 RMS AT/cm @Magnetic Field 0.300 T, Frequency 60 Hz | 0.0238 RMS VA/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0199 RMS AT/cm @Magnetic Field 0.400 T, Frequency 50 Hz | 0.0315 RMS VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0251 RMS AT/cm @Magnetic Field 0.400 T, Frequency 60 Hz | 0.0397 RMS VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0294 RMS AT/cm @Magnetic Field 0.500 T, Frequency 50 Hz | 0.0465 RMS VA/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0372 RMS AT/cm @Magnetic Field 0.500 T, Frequency 60 Hz | 0.0588 RMS VA/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0403 RMS AT/cm @Magnetic Field 0.600 T, Frequency 50 Hz | 0.0637 RMS VA/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0511 RMS AT/cm @Magnetic Field 0.600 T, Frequency 60 Hz | 0.0807 RMS VA/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.0528 RMS AT/cm @Magnetic Field 0.700 T, Frequency 50 Hz | 0.0834 RMS VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.06675 RMS AT/cm @Magnetic Field 0.800 T, Frequency 50 Hz | 0.1055 RMS VA/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.06700 RMS AT/cm @Magnetic Field 0.700 T, Frequency 60 Hz | 0.1059 RMS VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.08282 RMS AT/cm @Magnetic Field 0.900 T, Frequency 50 Hz | 0.1309 RMS VA/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.08485 RMS AT/cm @Magnetic Field 0.800 T, Frequency 60 Hz | 0.1341 RMS VA/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.1018 RMS AT/cm @Magnetic Field 1.00 T, Frequency 50 Hz | 0.1609 RMS VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.1055 RMS AT/cm @Magnetic Field 0.900 T, Frequency 60 Hz | 0.1668 RMS VA/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.1245 RMS AT/cm @Magnetic Field 1.10 T, Frequency 50 Hz | 0.1968 RMS VA/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.1294 RMS AT/cm @Magnetic Field 1.00 T, Frequency 60 Hz | 0.2045 RMS VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.1522 RMS AT/cm @Magnetic Field 1.20 T, Frequency 50 Hz | 0.2405 RMS VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.1585 RMS AT/cm @Magnetic Field 1.10 T, Frequency 60 Hz | 0.2505 RMS VA/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.1863 RMS AT/cm @Magnetic Field 1.30 T, Frequency 50 Hz | 0.2945 RMS VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.193 RMS AT/cm @Magnetic Field 1.20 T, Frequency 60 Hz | 0.305 RMS VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.2287 RMS AT/cm @Magnetic Field 1.40 T, Frequency 50 Hz | 0.3614 RMS VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.2356 RMS AT/cm @Magnetic Field 1.30 T, Frequency 60 Hz | 0.3723 RMS VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.2819 RMS AT/cm @Magnetic Field 1.50 T, Frequency 50 Hz | 0.4455 RMS VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.2876 RMS AT/cm @Magnetic Field 1.40 T, Frequency 60 Hz | 0.4545 RMS VA/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.3523 RMS AT/cm @Magnetic Field 1.50 T, Frequency 60 Hz | 0.5568 RMS VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.3532 RMS AT/cm @Magnetic Field 1.60 T, Frequency 50 Hz | 0.5582 RMS VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.4383 RMS AT/cm @Magnetic Field 1.60 T, Frequency 60 Hz | 0.6927 RMS VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.4774 RMS AT/cm @Magnetic Field 1.70 T, Frequency 50 Hz | 0.7545 RMS VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.5867 RMS AT/cm @Magnetic Field 1.70 T, Frequency 60 Hz | 0.9273 RMS VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 0.82536 RMS AT/cm @Magnetic Field 1.80 T, Frequency 50 Hz | 1.3045 RMS VA/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 1.0008 RMS AT/cm @Magnetic Field 1.80 T, Frequency 60 Hz | 1.5818 RMS VA/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 2.8558 RMS AT/cm @Magnetic Field 1.90 T, Frequency 50 Hz | 4.5136 RMS VA/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 3.5057 RMS AT/cm @Magnetic Field 1.90 T, Frequency 60 Hz | 5.5409 RMS VA/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
Electrical Resistivity | 0.0000500 ohm-cm | 0.0000500 ohm-cm |
|
Magnetic Properties | Metric | English | Comments |
---|
Core Loss | 0.00289 W/kg @Magnetic Field 0.100 T, Frequency 50 Hz | 0.00131 W/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00385 W/kg @Magnetic Field 0.100 T, Frequency 60 Hz | 0.00175 W/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.01082 W/kg @Magnetic Field 0.200 T, Frequency 50 Hz | 0.004908 W/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.01451 W/kg @Magnetic Field 0.200 T, Frequency 60 Hz | 0.006582 W/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0236 W/kg @Magnetic Field 0.300 T, Frequency 50 Hz | 0.0107 W/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0317 W/kg @Magnetic Field 0.300 T, Frequency 60 Hz | 0.0144 W/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0413 W/kg @Magnetic Field 0.400 T, Frequency 50 Hz | 0.0187 W/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0554 W/kg @Magnetic Field 0.400 T, Frequency 60 Hz | 0.0251 W/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0635 W/kg @Magnetic Field 0.500 T, Frequency 50 Hz | 0.0288 W/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0852 W/kg @Magnetic Field 0.500 T, Frequency 60 Hz | 0.0386 W/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0903 W/kg @Magnetic Field 0.600 T, Frequency 50 Hz | 0.0410 W/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.121 W/kg @Magnetic Field 0.600 T, Frequency 60 Hz | 0.0549 W/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.1218 W/kg @Magnetic Field 0.700 T, Frequency 50 Hz | 0.05525 W/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.1578 W/kg @Magnetic Field 0.800 T, Frequency 50 Hz | 0.07158 W/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.1628 W/kg @Magnetic Field 0.700 T, Frequency 60 Hz | 0.07384 W/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.1984 W/kg @Magnetic Field 0.900 T, Frequency 50 Hz | 0.08999 W/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.211 W/kg @Magnetic Field 0.800 T, Frequency 60 Hz | 0.0957 W/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.244 W/kg @Magnetic Field 1.00 T, Frequency 50 Hz | 0.111 W/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.265 W/kg @Magnetic Field 0.900 T, Frequency 60 Hz | 0.120 W/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.296 W/kg @Magnetic Field 1.10 T, Frequency 50 Hz | 0.134 W/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.325 W/kg @Magnetic Field 1.00 T, Frequency 60 Hz | 0.147 W/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.354 W/kg @Magnetic Field 1.20 T, Frequency 50 Hz | 0.161 W/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.394 W/kg @Magnetic Field 1.10 T, Frequency 60 Hz | 0.179 W/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.418 W/kg @Magnetic Field 1.30 T, Frequency 50 Hz | 0.190 W/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.470 W/kg @Magnetic Field 1.20 T, Frequency 60 Hz | 0.213 W/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.487 W/kg @Magnetic Field 1.40 T, Frequency 50 Hz | 0.221 W/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.555 W/kg @Magnetic Field 1.30 T, Frequency 60 Hz | 0.252 W/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.565 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz | 0.256 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.570 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz | 0.259 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.648 W/kg @Magnetic Field 1.40 T, Frequency 60 Hz | 0.294 W/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.655 W/kg @Magnetic Field 1.60 T, Frequency 50 Hz | 0.297 W/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.750 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz | 0.340 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.750 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz | 0.340 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.770 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | 0.349 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.773 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | 0.351 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.800 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | 0.363 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.867 W/kg @Magnetic Field 1.60 T, Frequency 60 Hz | 0.393 W/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.967 W/kg @Magnetic Field 1.80 T, Frequency 50 Hz | 0.439 W/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 1.01 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | 0.458 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.017 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | 0.4613 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.06 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | 0.481 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.264 W/kg @Magnetic Field 1.80 T, Frequency 60 Hz | 0.5733 W/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 1.365 W/kg @Magnetic Field 1.90 T, Frequency 50 Hz | 0.6192 W/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 1.766 W/kg @Magnetic Field 1.90 T, Frequency 60 Hz | 0.8010 W/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
|
Descriptive Properties |
---|
Approximate Equivalent International Grade | M080-23P5 |
Magnetostriction 10^8 | -18 |
| -20 |
| -20 |
| -21 |
Maximum Induction at 800 A/m (T) | 1.88 |
Minimum Lamination Factor (%) | 94.5 |
Typical Induction at 800 A/m (T) | 1.916 |
Typical Lamination Factor (%) | 96.6 |