MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Huntsman IROGRAN® A 85 H 4508 TPU-Polyester
Categories: Polymer; Thermoplastic; Polyurethane, TP; Thermoplastic Polyurethane (TPUR), Polyester Grade

Material Notes: Introduction: IROGRAN A 85 H 4508 is a thermoplastic polyester- polyurethane for injection molding applications. Additional characteristics of the product are excellent mechanical properties and high tear strength.

Performance Features:

  • Easy demolding
  • High production rates
  • Dynamically highly loadable
  • High demolding stability
  • Recyclable
Applications: For the production of mining screens, casual shoe soles conveyor rollers, top lifts, wheels and rollers

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.17 g/ccInjection molded parts
Linear Mold Shrinkage 0.0050 in/inInjection molded; ASTM D955
Melt Index of Compound 50 g/10 min
@Load 21.6 kg,
Temperature 190 °C
MVR, [cm3/10 min]
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 85Injection molded parts; ASTM D2240
Hardness, Shore D 34Injection molded parts; ASTM D2240
Tensile Strength at Break 40.0 MPaInjection molded parts; DIN 53504
Elongation at Break 650 %Injection molded parts; DIN 53504
100% Modulus 0.00600 GPa
@Strain 100 %
Injection molded parts; DIN 53504
300% Modulus 0.0130 GPa
@Strain 300 %
Injection molded parts; DIN 53504
Tear Strength 399 pliInjection molded parts; DIN 53515
Abrasion 30mm3, Injection molded; DIN 53516
Compression Set 25 %
@Temperature 22.8 °C,
Time 86400 sec
Injection molded; ASTM D395
 40 %
@Temperature 70.0 °C,
Time 86400 sec
Injection molded; ASTM D395
 
Thermal PropertiesOriginal ValueComments
Melting Point 137 - 200 °C
 
Processing PropertiesOriginal ValueComments
Feed Temperature 25.0 - 40.0 °CExtrusion
Middle Barrel Temperature 165 - 190 °CExtrusion
Nozzle Temperature 170 - 200 °CExtrusion
 180 - 200 °CInjection
Adapter Temperature 175 - 195 °CExtrusion
Die Temperature 175 - 200 °CExtrusion
Melt Temperature 170 - 195 °CInjection
Mold Temperature 20.0 - 70.0 °CInjection
 
Descriptive Properties
Heating Zone175-195°CInjection

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Lubrizol LifeSciences Pellethane® 5863-80A TPU
Lubrizol ESTANE® 58219 Ether Based Thermoplastic Polyurethane
Lubrizol Advanced Materials Pearlthane® ECO D12T90E Thermoplastic Polyurethane
Lubrizol Advanced Materials Pearlthane® ECO D12T85 Thermoplastic Polyurethane
Lubrizol Advanced Materials Pearlthane® 11T75D Thermoplastic Polyurethane Elastomer

PHUQ096 / 159469

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.