Physical Properties | Metric | English | Comments |
---|
Density | 7.81 g/cc | 0.282 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Brinell | 163 @Diameter 19.0 - 25.4 mm | 163 @Diameter 0.750 - 1.00 in |
| 167 @Diameter 12.7 mm | 167 @Diameter 0.500 in |
| 241 @Diameter 3.17 mm | 241 @Diameter 0.125 in |
| 251 @Diameter 4.762 mm | 251 @Diameter 0.1875 in |
| 251 @Diameter 9.52 mm | 251 @Diameter 0.375 in |
| 256 @Diameter 0.838 - 2.10 mm | 256 @Diameter 0.0330 - 0.0825 in |
| 256 @Diameter 6.35 mm | 256 @Diameter 0.250 in |
Hardness, Knoop | 255 @Diameter 3.17 mm | 255 @Diameter 0.125 in |
| 266 @Diameter 4.762 mm | 266 @Diameter 0.1875 in |
| 266 @Diameter 9.52 mm | 266 @Diameter 0.375 in |
| 271 @Diameter 6.35 mm | 271 @Diameter 0.250 in |
| 271 @Diameter 0.838 - 2.10 mm | 271 @Diameter 0.0330 - 0.0825 in |
Hardness, Rockwell B | 95 @Diameter 19.0 - 25.4 mm | 95 @Diameter 0.750 - 1.00 in |
| 97 @Diameter 12.7 mm | 97 @Diameter 0.500 in |
Hardness, Rockwell C | 21 @Diameter 3.17 mm | 21 @Diameter 0.125 in |
| 23 @Diameter 4.762 mm | 23 @Diameter 0.1875 in |
| 23 @Diameter 9.52 mm | 23 @Diameter 0.375 in |
| 24 @Diameter 6.35 mm | 24 @Diameter 0.250 in |
| 24 @Diameter 0.838 - 2.10 mm | 24 @Diameter 0.0330 - 0.0825 in |
Hardness, Vickers | 220 @Diameter 19.0 - 25.4 mm | 220 @Diameter 0.750 - 1.00 in |
| 233 @Diameter 12.7 mm | 233 @Diameter 0.500 in |
| 247 @Diameter 3.17 mm | 247 @Diameter 0.125 in |
| 258 @Diameter 4.762 mm | 258 @Diameter 0.1875 in |
| 258 @Diameter 9.52 mm | 258 @Diameter 0.375 in |
| 263 @Diameter 6.35 mm | 263 @Diameter 0.250 in |
| 263 @Diameter 0.838 - 2.10 mm | 263 @Diameter 0.0330 - 0.0825 in |
Tensile Strength, Ultimate | 800 MPa @Diameter 19.0 - 25.4 mm | 116000 psi @Diameter 0.750 - 1.00 in |
| 834 MPa @Diameter 12.7 mm | 121000 psi @Diameter 0.500 in |
| 841 MPa @Diameter 6.35 mm | 122000 psi @Diameter 0.250 in |
| 841 MPa @Diameter 9.52 mm | 122000 psi @Diameter 0.375 in |
| 855 MPa @Diameter 3.17 mm | 124000 psi @Diameter 0.125 in |
| 869 MPa @Diameter 4.762 mm | 126000 psi @Diameter 0.1875 in |
| 896 MPa @Diameter 0.838 - 2.10 mm | 130000 psi @Diameter 0.0330 - 0.0825 in |
Tensile Strength, Yield | 600 MPa @Diameter 19.0 - 25.4 mm, Strain 0.2 % | 87000 psi @Diameter 0.750 - 1.00 in, Strain 0.2 % |
| 600 MPa @Strain 0.2 %, Diameter 12.7 mm | 87000 psi @Strain 0.2 %, Diameter 0.500 in |
| 627 MPa @Strain 0.2 %, Diameter 9.52 mm | 90900 psi @Strain 0.2 %, Diameter 0.375 in |
| 641 MPa @Strain 0.2 %, Diameter 6.35 mm | 93000 psi @Strain 0.2 %, Diameter 0.250 in |
| 648 MPa @Diameter 3.17 mm, Strain 0.2 % | 94000 psi @Diameter 0.125 in, Strain 0.2 % |
| 662 MPa @Diameter 4.762 mm, Strain 0.2 % | 96000 psi @Diameter 0.1875 in, Strain 0.2 % |
| 683 MPa @Diameter 0.838 - 2.10 mm, Strain 0.2 % | 99100 psi @Diameter 0.0330 - 0.0825 in, Strain 0.2 % |
Elongation at Break | 25 % @Diameter 0.838 - 2.10 mm | 25 % @Diameter 0.0330 - 0.0825 in |
| 25 % @Diameter 3.17 mm | 25 % @Diameter 0.125 in |
| 25 % @Diameter 4.762 mm | 25 % @Diameter 0.1875 in |
| 27 % @Diameter 6.35 mm | 27 % @Diameter 0.250 in |
| 31 % @Diameter 9.52 mm | 31 % @Diameter 0.375 in |
| 31 % @Diameter 19.0 - 25.4 mm | 31 % @Diameter 0.750 - 1.00 in |
| 34 % @Diameter 12.7 mm | 34 % @Diameter 0.500 in |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.0000840 ohm-cm @Temperature 25.0 °C | 0.0000840 ohm-cm @Temperature 77.0 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 10.6 µm/m-°C @Temperature 22.0 - 95.0 °C | 5.89 µin/in-°F @Temperature 71.6 - 203 °F |
| 10.8 µm/m-°C @Temperature 22.0 - 150 °C | 6.00 µin/in-°F @Temperature 71.6 - 302 °F |
| 11.2 µm/m-°C @Temperature 22.0 - 205 °C | 6.22 µin/in-°F @Temperature 71.6 - 401 °F |
| 12.1 µm/m-°C @Temperature 20.0 - 315 °C | 6.72 µin/in-°F @Temperature 68.0 - 599 °F |
| 12.4 µm/m-°C @Temperature 20.0 - 425 °C | 6.89 µin/in-°F @Temperature 68.0 - 797 °F |
| 13.0 µm/m-°C @Temperature 20.0 - 540 °C | 7.22 µin/in-°F @Temperature 68.0 - 1000 °F |
Specific Heat Capacity | 0.480 J/g-°C | 0.115 BTU/lb-°F |
Thermal Conductivity | 15.1 W/m-K @Temperature 100 °C | 105 BTU-in/hr-ft²-°F @Temperature 212 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Carbon, C | <= 0.040 % | <= 0.040 % |
Chromium, Cr | 26 % | 26 % |
Copper, Cu | 1.7 % | 1.7 % |
Iron, Fe | 62 % | 62 % |
Manganese, Mn | 0.80 % | 0.80 % |
Molybdenum, Mo | 3.3 % | 3.3 % |
Nickel, Ni | 5.5 % | 5.5 % |
Nitrogen, N | 0.17 % | 0.17 % |
Silicon, Si | 0.45 % | 0.45 % |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.