MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Ferralium Alloy 255 solution heat treated, hardened at 510°C (950°F) for 4 hours
Categories: Metal; Ferrous Metal; Heat Resisting; Stainless Steel

Material Notes: Patented, ferritic-austenitic; high mechanical strength, ductility, and hardness with resistance to corrosion and erosion. Excellent resistance to acids and salts. Duplex alloy with nearly equal portions of austenite and ferrite-matrix phases. Applications include pumps, agitators, valves, and piping for handling wet phosphoric acid slurries, marine scrubbers, pumps and seals, and acid handling equipment.

Key Words: UNS S32550
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.81 g/cc0.282 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell  304
@Diameter 12.7 mm
304
@Diameter 0.500 in
Converted from Rockwell C hardness.
 326
@Diameter 6.35 mm
326
@Diameter 0.250 in
Converted from Rockwell C hardness.
Hardness, Knoop  326
@Diameter 12.7 mm
326
@Diameter 0.500 in
Converted from Rockwell C hardness.
 352
@Diameter 6.35 mm
352
@Diameter 0.250 in
Converted from Rockwell C hardness.
Hardness, Rockwell C  32
@Diameter 12.7 mm
32
@Diameter 0.500 in
 35
@Diameter 6.35 mm
35
@Diameter 0.250 in
Hardness, Vickers  316
@Diameter 12.7 mm
316
@Diameter 0.500 in
Converted from Rockwell C hardness.
 340
@Diameter 6.35 mm
340
@Diameter 0.250 in
Converted from Rockwell C hardness.
Tensile Strength, Ultimate  855 MPa
@Diameter 6.35 mm
124000 psi
@Diameter 0.250 in
 876 MPa
@Diameter 12.7 mm
127000 psi
@Diameter 0.500 in
 883 MPa
@Diameter 9.52 mm
128000 psi
@Diameter 0.375 in
 903 MPa
@Diameter 3.17 mm
131000 psi
@Diameter 0.125 in
 910 MPa
@Diameter 4.762 mm
132000 psi
@Diameter 0.1875 in
 938 MPa
@Diameter 19.0 - 25.4 mm
136000 psi
@Diameter 0.750 - 1.00 in
 979 MPa
@Diameter 0.838 - 2.10 mm
142000 psi
@Diameter 0.0330 - 0.0825 in
Tensile Strength, Yield  641 MPa
@Strain 0.2 %,
Diameter 12.7 mm
93000 psi
@Strain 0.2 %,
Diameter 0.500 in
 683 MPa
@Strain 0.2 %,
Diameter 6.35 mm
99100 psi
@Strain 0.2 %,
Diameter 0.250 in
 683 MPa
@Strain 0.2 %,
Diameter 9.52 mm
99100 psi
@Strain 0.2 %,
Diameter 0.375 in
 689 MPa
@Diameter 4.762 mm,
Strain 0.2 %
99900 psi
@Diameter 0.1875 in,
Strain 0.2 %
 703 MPa
@Diameter 3.17 mm,
Strain 0.2 %
102000 psi
@Diameter 0.125 in,
Strain 0.2 %
 717 MPa
@Diameter 19.0 - 25.4 mm,
Strain 0.2 %
104000 psi
@Diameter 0.750 - 1.00 in,
Strain 0.2 %
 772 MPa
@Diameter 0.838 - 2.10 mm,
Strain 0.2 %
112000 psi
@Diameter 0.0330 - 0.0825 in,
Strain 0.2 %
Elongation at Break  22 %
@Diameter 0.838 - 2.10 mm
22 %
@Diameter 0.0330 - 0.0825 in
in 50 mm
 24 %
@Diameter 3.17 mm
24 %
@Diameter 0.125 in
in 50 mm
 24 %
@Diameter 4.762 mm
24 %
@Diameter 0.1875 in
in 50 mm
 26 %
@Diameter 6.35 mm
26 %
@Diameter 0.250 in
in 50 mm
 28 %
@Diameter 19.0 - 25.4 mm
28 %
@Diameter 0.750 - 1.00 in
in 50 mm
 30 %
@Diameter 9.52 mm
30 %
@Diameter 0.375 in
in 50 mm
 31 %
@Diameter 12.7 mm
31 %
@Diameter 0.500 in
in 50 mm
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000840 ohm-cm
@Temperature 25.0 °C
0.0000840 ohm-cm
@Temperature 77.0 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.0 µm/m-°C
@Temperature 20.0 - 93.0 °C
6.11 µin/in-°F
@Temperature 68.0 - 199 °F
 11.7 µm/m-°C
@Temperature 20.0 - 205 °C
6.50 µin/in-°F
@Temperature 68.0 - 401 °F
 12.1 µm/m-°C
@Temperature 20.0 - 315 °C
6.72 µin/in-°F
@Temperature 68.0 - 599 °F
 12.4 µm/m-°C
@Temperature 20.0 - 425 °C
6.89 µin/in-°F
@Temperature 68.0 - 797 °F
 13.0 µm/m-°C
@Temperature 20.0 - 540 °C
7.22 µin/in-°F
@Temperature 68.0 - 1000 °F
Specific Heat Capacity 0.480 J/g-°C0.115 BTU/lb-°FTypical value for stainless steel.
Thermal Conductivity 15.1 W/m-K
@Temperature 100 °C
105 BTU-in/hr-ft²-°F
@Temperature 212 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.040 %<= 0.040 %
Chromium, Cr 26 %26 %
Copper, Cu 1.7 %1.7 %
Iron, Fe 62 %62 %
Manganese, Mn 0.80 %0.80 %
Molybdenum, Mo 3.3 %3.3 %
Nickel, Ni 5.5 %5.5 %
Nitrogen, N 0.17 %0.17 %
Silicon, Si 0.45 %0.45 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Ferralium Alloy 255 solution treated at 1120°C, cooled rapidly
ATI Allegheny Ludlum Alloy 255 Duplex Stainless Steel, UNS S32550
Sandvik SAF 2507 Plate, Sheet and Coil
AK Steel 2205 Duplex Stainless steel
Ferralium Alloy 255 heat treated at 1120°C, cooled rapidly, 10.2-19 mm thick plate

MQN255H / 13875

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.