MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Overview of materials for Thermoplastic Polyurethane, Elastomer, Polyester Grade
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyurethane, TP; Thermoplastic Polyurethane, Elastomer, Polyester Grade

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Thermoplastic Polyurethane, Elastomer, Polyester Grade". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 0.992 - 1.44 g/ccAverage value: 1.21 g/cc Grade Count:282
Viscosity 30.0 - 5500 cPAverage value: 1010 cP Grade Count:18
 28000 - 130000 cP
@Temperature 204 - 204 °C
Average value: 83800 cP Grade Count:4
Maximum Moisture Content 0.0200 - 0.0500Average value: 0.0332 Grade Count:34
Linear Mold Shrinkage 0.00200 - 0.0250 cm/cmAverage value: 0.00758 cm/cm Grade Count:73
Linear Mold Shrinkage, Transverse -0.00200 - 0.00900 cm/cmAverage value: 0.00496 cm/cm Grade Count:12
Melt Flow 5.00 - 90.0 g/10 minAverage value: 34.1 g/10 min Grade Count:46
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 40.0 - 101Average value: 84.8 Grade Count:225
Hardness, Shore D 12.0 - 79.0Average value: 50.5 Grade Count:124
Tensile Strength, Ultimate 3.45 - 72.1 MPaAverage value: 39.4 MPa Grade Count:277
Tensile Strength, Yield 20.0 - 42.1 MPaAverage value: 36.3 MPa Grade Count:5
Elongation at Break 10.0 - 1580 %Average value: 565 % Grade Count:282
Modulus of Elasticity 0.00300 - 0.870 GPaAverage value: 0.147 GPa Grade Count:25
Flexural Yield Strength 2.61 - 62.7 MPaAverage value: 24.3 MPa Grade Count:6
Flexural Modulus 0.0276 - 1.21 GPaAverage value: 0.234 GPa Grade Count:26
Resilience 30.0 - 60.0Average value: 42.3 Grade Count:22
Rebound 25.0 - 57.0 %Average value: 37.9 % Grade Count:39
Shear Modulus 0.0120 - 0.250 GPaAverage value: 0.102 GPa Grade Count:3
Izod Impact, Notched 0.854 - 5340 J/cmAverage value: 4.63 J/cm Grade Count:6
 0.26695 - 2.93645 J/cm
@Temperature -40.0 - -40.0 °C
Average value: 1.60 J/cm Grade Count:2
Izod Impact, Unnotched 0.961 - 5340 J/cmAverage value: 0.961 J/cm Grade Count:3
Tear Strength 17.5 - 333 kN/mAverage value: 116 kN/m Grade Count:256
Peel Strength 0.0400 - 7.20 kN/mAverage value: 1.93 kN/m Grade Count:6
Graves Tear Strength 52.6 - 210 kN/mAverage value: 127 kN/m Grade Count:20
Taber Abrasion, mg/1000 Cycles 2.50 - 127Average value: 37.9 Grade Count:87
Compression Set 12.0 - 90.0 %Average value: 35.4 % Grade Count:110
Tensile Set 4.00 - 155 %Average value: 52.8 % Grade Count:46
 20.0 - 20.0 %
@Temperature 200 - 200 °C
Average value: 20.0 % Grade Count:1
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 1.00e+10 - 1.00e+13 ohm-cmAverage value: 3.37e+12 ohm-cm Grade Count:3
Surface Resistance 5.00e+8 - 1.00e+12 ohmAverage value: 2.78e+11 ohm Grade Count:4
Dielectric Constant 4.10 - 7.10Average value: 5.73 Grade Count:3
Dielectric Strength 31.0 - 49.0 kV/mmAverage value: 42.7 kV/mm Grade Count:3
Dissipation Factor 0.0240 - 0.200Average value: 0.0557 Grade Count:3
Comparative Tracking Index 600 VAverage value: 600 V Grade Count:6
 
Thermal PropertiesOriginal ValueComments
CTE, linear 117 - 171 µm/m-°CAverage value: 150 µm/m-°C Grade Count:15
Melting Point 100 - 230 °CAverage value: 167 °C Grade Count:44
Vicat Softening Point 35.0 - 165 °CAverage value: 106 °C Grade Count:79
Brittleness Temperature -70.0 - -50.0 °CAverage value: -66.4 °C Grade Count:7
Glass Transition Temp, Tg -47.0 - 120 °CAverage value: -21.8 °C Grade Count:41
Transformation Temperature -27.8 - -17.2 °CAverage value: -22.0 °C Grade Count:3
Clash Berg Stiffness Temperature -40.0 - -5.00 °CAverage value: -26.4 °C Grade Count:6
Flammability, UL94 HBGrade Count:3
Ring & Ball Softening Point 161 - 179 °CAverage value: 170 °C Grade Count:3
 
Optical PropertiesOriginal ValueComments
Haze 1.10 %Average value: 1.10 % Grade Count:3
Transmission, Visible 90.0 %Average value: 90.0 % Grade Count:11
 
Processing PropertiesOriginal ValueComments
Processing Temperature 155 - 230 °CAverage value: 196 °C Grade Count:60
Nozzle Temperature 160 - 299 °CAverage value: 200 °C Grade Count:80
Adapter Temperature 175 - 215 °CAverage value: 193 °C Grade Count:46
Die Temperature 145 - 215 °CAverage value: 194 °C Grade Count:59
Melt Temperature 120 - 238 °CAverage value: 192 °C Grade Count:111
Head Temperature 170 - 210 °CAverage value: 195 °C Grade Count:10
Mold Temperature 10.0 - 70.0 °CAverage value: 35.7 °C Grade Count:53
Drying Temperature 54.0 - 110 °CAverage value: 98.5 °C Grade Count:96
Moisture Content 0.0100 - 0.100 %Average value: 0.0395 % Grade Count:19
Dew Point -40.0 - -30.0 °CAverage value: -35.8 °C Grade Count:36
Injection Pressure 4.96 - 15000 MPaAverage value: 958 MPa Grade Count:13

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Thermoplastic Polyurethane, Elastomer, Ether Grade
Overview of materials for Thermoset Polyurethane, Elastomer, Unreinforced
Overview of materials for Thermoplastic Polyurethane, Elastomer, Glass Filled
Overview of materials for Thermoplastic Polyurethane (TPUR), Polyester Grade
Overview of materials for Polyester Thermoplastic Elastomer

O5033 / 78462

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.