MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Thermoplastic Polyurethane (TPUR), Polyester Grade
Categories: Polymer; Thermoplastic; Polyurethane, TP; Thermoplastic Polyurethane (TPUR), Polyester Grade

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Thermoplastic Polyurethane (TPUR), Polyester Grade". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 0.650 - 1.44 g/cc0.0235 - 0.0520 lb/in³Average value: 1.20 g/cc Grade Count:413
Particle Size 50.0 - 500 µm50.0 - 500 µmAverage value: 275 µm Grade Count:9
pH 7.00 - 9.507.00 - 9.50Average value: 8.17 Grade Count:3
Viscosity 20.0 - 25000 cP20.0 - 25000 cPAverage value: 3240 cP Grade Count:36
 223000 - 223000 cP
@Temperature 204 - 204 °C
223000 - 223000 cP
@Temperature 399 - 399 °F
Average value: 223000 cP Grade Count:1
Maximum Moisture Content 0.0200 - 0.1000.0200 - 0.100Average value: 0.0429 Grade Count:16
Linear Mold Shrinkage 0.000700 - 0.0300 cm/cm0.000700 - 0.0300 in/inAverage value: 0.00871 cm/cm Grade Count:45
Melt Flow 5.00 - 112 g/10 min5.00 - 112 g/10 minAverage value: 38.4 g/10 min Grade Count:81
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 30.0 - 10130.0 - 101Average value: 84.3 Grade Count:464
 74.0 - 75.0
@Temperature 70.0 - 100 °C
74.0 - 75.0
@Temperature 158 - 212 °F
Average value: 74.5 Grade Count:1
Hardness, Shore D 15.0 - 92.015.0 - 92.0Average value: 52.9 Grade Count:189
Tensile Strength, Ultimate 0.785 - 80.0 MPa114 - 11600 psiAverage value: 35.6 MPa Grade Count:507
 4.05 - 26.63 MPa
@Temperature 70.0 - 100 °C
587 - 3862 psi
@Temperature 158 - 212 °F
Average value: 31.2 MPa Grade Count:1
 25.0 - 35.0 MPa
@Temperature 80.0 - 80.0 °C
3630 - 5080 psi
@Temperature 176 - 176 °F
Average value: 31.2 MPa Grade Count:7
 25.0 - 35.0 MPa
@Time 1.81e+6 - 1.81e+6 sec
3630 - 5080 psi
@Time 504 - 504 hour
Average value: 31.2 MPa Grade Count:7
 30.0 - 65.0 MPa
@Strain 2.00 - 2.00 %
4350 - 9430 psi
@Strain 2.00 - 2.00 %
Average value: 31.2 MPa Grade Count:1
 30.0 - 65.0 MPa
@Temperature 0.000 - 60.0 °C
4350 - 9430 psi
@Temperature 32.0 - 140 °F
Average value: 31.2 MPa Grade Count:1
Tensile Strength, Yield 1.00 - 59.2 MPa145 - 8590 psiAverage value: 21.1 MPa Grade Count:68
Elongation at Break 10.0 - 1100 %10.0 - 1100 %Average value: 549 % Grade Count:497
 690 - 1080 %
@Temperature 70.0 - 100 °C
690 - 1080 %
@Temperature 158 - 212 °F
Average value: 538 % Grade Count:1
 450 - 530 %
@Temperature 80.0 - 80.0 °C
450 - 530 %
@Temperature 176 - 176 °F
Average value: 538 % Grade Count:7
 450 - 530 %
@Time 1.81e+6 - 1.81e+6 sec
450 - 530 %
@Time 504 - 504 hour
Average value: 538 % Grade Count:7
Elongation at Yield 320 - 850 %320 - 850 %Average value: 537 % Grade Count:36
Modulus of Elasticity 0.00500 - 1.90 GPa0.725 - 276 ksiAverage value: 0.470 GPa Grade Count:15
 0.0240 - 1.75 GPa
@Temperature -20.0 - 60.0 °C
3.48 - 254 ksi
@Temperature -4.00 - 140 °F
Average value: 0.522 GPa Grade Count:2
Flexural Modulus 0.00383 - 0.830 GPa0.555 - 120 ksiAverage value: 0.126 GPa Grade Count:20
Resilience 20.0 - 55.020.0 - 55.0Average value: 35.1 Grade Count:43
Rebound 1.21 - 60.0 %1.21 - 60.0 %Average value: 39.2 % Grade Count:26
Izod Impact, Notched 0.640 - 0.850 J/cm
@Temperature -40.0 - -40.0 °C
1.20 - 1.59 ft-lb/in
@Temperature -40.0 - -40.0 °F
Average value: 0.745 J/cm Grade Count:2
Izod Impact, Notched (ISO) NBNBGrade Count:16
 35.0 - 125 kJ/m²
@Temperature -30.0 - -30.0 °C
16.7 - 59.5 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 79.1 kJ/m² Grade Count:7
Izod Impact, Unnotched (ISO) NBNBGrade Count:16
 55.0 - 205 kJ/m²
@Temperature -30.0 - -30.0 °C
26.2 - 97.5 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 130 kJ/m² Grade Count:7
Charpy Impact Unnotched 10.0 - 1000 J/cm²47.6 - 4760 ft-lb/in²Average value: 13.4 J/cm² Grade Count:9
 7.00 - 16.0 J/cm²
@Temperature -30.0 - -30.0 °C
33.3 - 76.1 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 10.2 J/cm² Grade Count:9
Charpy Impact, Notched 3.00 - 1000 J/cm²14.3 - 4760 ft-lb/in²Average value: 6.73 J/cm² Grade Count:47
 0.300 - 999.9 J/cm²
@Temperature -30.0 - -30.0 °C
1.43 - 4759 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 3.72 J/cm² Grade Count:47
Tear Strength 5.43 - 312 kN/m31.0 - 1780 pliAverage value: 114 kN/m Grade Count:425
Graves Tear Strength 29.8 - 154 kN/m170 - 880 pliAverage value: 78.0 kN/m Grade Count:5
K Factor (Wear Factor) 30.0 - 80.030.0 - 80.0Average value: 51.8 Grade Count:36
Taber Abrasion, mg/1000 Cycles 1.40 - 1461.40 - 146Average value: 30.2 Grade Count:44
Compression Set 10.0 - 102 %10.0 - 102 %Average value: 36.3 % Grade Count:239
Tensile Set 4.00 - 19.0 %4.00 - 19.0 %Average value: 12.1 % Grade Count:5
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 8.00e+11 - 5.00e+14 ohm-cm8.00e+11 - 5.00e+14 ohm-cmAverage value: 1.03e+14 ohm-cm Grade Count:5
Surface Resistance 1.00e+8 - 9.00e+14 ohm1.00e+8 - 9.00e+14 ohmAverage value: 1.13e+14 ohm Grade Count:8
Dielectric Constant 3.90 - 6.503.90 - 6.50Average value: 5.15 Grade Count:5
Dielectric Strength 14.1 - 23.7 kV/mm358 - 602 kV/inAverage value: 18.5 kV/mm Grade Count:5
Dissipation Factor 0.0240 - 0.08400.0240 - 0.0840Average value: 0.0449 Grade Count:5
 
Thermal PropertiesMetricEnglishComments
CTE, linear 15.0 - 210 µm/m-°C8.33 - 117 µin/in-°FAverage value: 88.2 µm/m-°C Grade Count:16
Melting Point 71.0 - 221 °C160 - 430 °FAverage value: 151 °C Grade Count:74
Maximum Service Temperature, Air 100 °C212 °FAverage value: 100 °C Grade Count:16
Deflection Temperature at 0.46 MPa (66 psi) 51.0 - 170 °C124 - 338 °FAverage value: 124 °C Grade Count:12
Deflection Temperature at 1.8 MPa (264 psi) 48.0 - 130 °C118 - 266 °FAverage value: 97.2 °C Grade Count:12
Vicat Softening Point 38.0 - 163 °C100 - 325 °FAverage value: 99.7 °C Grade Count:85
Softening Point 60.0 - 185 °C140 - 365 °FAverage value: 123 °C Grade Count:38
Minimum Service Temperature, Air -50.0 °C-58.0 °FAverage value: -50.0 °C Grade Count:16
Glass Transition Temp, Tg -48.3 - -5.00 °C-55.0 - 23.0 °FAverage value: -30.3 °C Grade Count:104
Flammability, UL94 HB - V-2HB - V-2Grade Count:4
Ring & Ball Softening Point 71.0 - 184 °C160 - 363 °FAverage value: 106 °C Grade Count:7
 
Optical PropertiesMetricEnglishComments
Transmission, Visible 90.0 %90.0 %Average value: 90.0 % Grade Count:11
 
Processing PropertiesMetricEnglishComments
Processing Temperature 50.0 - 245 °C122 - 473 °FAverage value: 190 °C Grade Count:143
Nozzle Temperature 150 - 235 °C302 - 455 °FAverage value: 196 °C Grade Count:89
Adapter Temperature 150 - 230 °C302 - 446 °FAverage value: 193 °C Grade Count:71
Die Temperature 150 - 235 °C302 - 455 °FAverage value: 194 °C Grade Count:97
Melt Temperature 87.8 - 245 °C190 - 473 °FAverage value: 195 °C Grade Count:137
Mold Temperature 10.0 - 70.0 °C50.0 - 158 °FAverage value: 38.9 °C Grade Count:135
Roll Temperature 115 - 180 °C239 - 356 °FAverage value: 158 °C Grade Count:7
Drying Temperature 70.0 - 150 °C158 - 302 °FAverage value: 90.1 °C Grade Count:45
Moisture Content 0.0500 - 0.100 %0.0500 - 0.100 %Average value: 0.0897 % Grade Count:34
Dew Point -40.0 - -30.0 °C-40.0 - -22.0 °FAverage value: -35.3 °C Grade Count:20
Injection Pressure 2.00 - 103 MPa290 - 14900 psiAverage value: 12.2 MPa Grade Count:63
Cycle Time - Injection 2.50 - 45.0 sec2.50 - 45.0 secAverage value: 26.7 sec Grade Count:22
Cycle Time - Cooling 30.0 - 38.0 sec30.0 - 38.0 secAverage value: 35.3 sec Grade Count:3
Cure Time 1.00 - 480 min0.0167 - 8.00 hourAverage value: 43.3 min Grade Count:33

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Thermoplastic Polyurethane (TPUR), Polyether Grade
Overview of materials for Thermoplastic Polyurethane, Elastomer, Polyester Grade
Overview of materials for Thermoplastic Polyurethane, Elastomer, Ether Grade
Natural Rubber, Vulcanized (NR, IR, Polyisoprene)
Natural Rubber, Not Vulcanized (NR, IR, Polyisoprene)

O5040 / 78463

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.