MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Envalior Pocan® B 1300 000000 PBT
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Unreinforced, Molded

Material Notes: PBT, non-reinforced, injection molding, extrusion

Former Lanxess product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Bulk Density 0.800 g/ccISO 60
Density 1.30 g/ccISO 1183
Moisture Absorption at Equilibrium 0.20 %50% RH; ISO 62
Water Absorption at Saturation 0.50 %ISO 62
Viscosity Test 105 cm³/gViscosity Number; ISO 1628-5
Linear Mold Shrinkage, Flow 0.019 cm/cm150x105x3; 260 °C / MT 80 °C; 600 bar; ISO 2577
Linear Mold Shrinkage, Transverse 0.019 cm/cm150x105x3; 260 °C / MT 80 °C; 600 bar; ISO 2577
Melt Flow 45 g/10 min
@Load 2.16 kg,
Temperature 250 °C
ISO 1133-1
 
Mechanical PropertiesOriginal ValueComments
Puncture Resistance 3800 N
@Temperature -30.0 °C
ISO 6603-2
Ball Indentation Hardness 120 MPaISO 2093-1
Tensile Strength, Yield 55.0 MPa50 mm/min; ISO 527-1,-2
Elongation at Break >= 20 %50 mm/min, Nominal; ISO 527-1,-2
Elongation at Yield 8.0 %50 mm/min; ISO 527-1,-2
Tensile Modulus 2700 MPa1 mm/min; ISO 527-1,-2
Flexural Strength 90.0 MPa2 mm/min; ISO 178-A
Flexural Yield Strength 75.0 MPa
@Strain 3.5 %
2 mm/min; ISO 178-A
Flexural Modulus 2700 MPa2 mm/min; ISO 178-A
Flexural Strain at Break 6.0 %2 mm/min; ISO 178-A
Izod Impact, Notched (ISO) <= 10.0 kJ/m²
@Temperature 23.0 °C
ISO 180-1A
 <= 10.0 kJ/m²
@Temperature -30.0 °C
ISO 180-1A
 <= 10.0 kJ/m²
@Temperature -40.0 °C
ISO 180-1A
Izod Impact, Unnotched (ISO) 150 kJ/m²
@Temperature 23.0 °C
ISO 180-1U
 150 kJ/m²
@Temperature -30.0 °C
ISO 180-1U
Charpy Impact Unnotched 150 kJ/m²
@Temperature -30.0 °C
ISO 179-1eU
 220 kJ/m²
@Temperature 23.0 °C
ISO 179-1eU
Charpy Impact, Notched <= 10.0 kJ/m²
@Temperature 23.0 °C
ISO 179 1eA
 <= 10.0 kJ/m²
@Temperature -30.0 °C
ISO 179 1eA
Puncture Energy 15.0 J
@Temperature -30.0 °C
ISO 6603-2
 40.0 J
@Temperature 23.0 °C
ISO 6603-2
Tensile Creep Modulus, 1 hour 2400 MPaISO 899-1
Tensile Creep Modulus, 1000 hours 1400 MPaISO 899-1
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 3.2
@Frequency 1e+6 Hz
IEC 60250
 3.4
@Frequency 100 Hz
IEC 60250
Dielectric Strength 28.0 kV/mm
@Thickness 1.00 mm
IEC 60243-1
Comparative Tracking Index 300 VSolution B; IEC 60112
 600 VSolution A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 120 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1,-2
CTE, linear, Transverse to Flow 130 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1,-2
Thermal Conductivity 0.250 W/m-KISO 8302
Melting Point 225 °C10°C/min; ISO 11357-1,-3
Maximum Service Temperature, Air 190 °CIEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi) 160 °CISO 75-1,-2
Deflection Temperature at 1.8 MPa (264 psi) 60.0 °CISO 75-1,-2
Deflection Temperature at 8.0 MPa 45.0 °CISO 75-1,-2
Vicat Softening Point 180 °C
@Load 5.10 kg
50°C/h; ISO 306
Flammability, UL94 HB
@Thickness 0.800 mm
 HB
@Thickness 1.60 mm
Oxygen Index 24 %Method A; ISO 4589-2
Glow Wire Flammability Index 750 °C
@Thickness 2.00 mm
IEC 60695-2-12
Shrinkage, MD 0.50 %
@Treatment Temp. 150 °C,
Time 3600 sec
Flow Direction Post-Molding, 150x105x3; ISO 2577
Shrinkage, TD 0.50 %
@Treatment Temp. 150 °C,
Time 3600 sec
Post-Molding, 150x105x3; ISO 2577
 
Processing PropertiesOriginal ValueComments
Melt Temperature 260 °Cinjection molding; ISO 294
Mold Temperature 80.0 °Cinjection molding; ISO 294
Drying Temperature 120 °C
Dry Time 4.00 - 8.00 hour
Moisture Content 0.00 - 0.020 %Karl Fischer

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Lanxess Pocan® B 700 000000 PBT
Envalior Pocan® DP 1105 000000 PBT
Envalior Pocan® B 1700 000000 PBT
Envalior Pocan® B 1305 000000 PBT
Envalior Pocan® B 1100 000000 PBT

PLANW9187 / 208388

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.