MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

DuPont Mobility and Materials Crastin® T835FRUV NC010 PBT  (discontinued **)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), 10% Glass Fiber Filled

Material Notes: Crastin® T835FRUV NC010 is a 5% glass fiber reinforced, toughened, flame retardant polybutylene terephthalate resin for injection molding. (precommercial code = Crastin® CE2402)

While this product line has been acquired by Celanese, this specific grade had been disconued while still a DuPont product so it is listed here as a discontinued DuPont product.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.43 g/cc0.0517 lb/in³ISO 1183
Filler Content 5.0 %5.0 %
Linear Mold Shrinkage 0.013 cm/cm
@Thickness 3.20 mm
0.013 in/in
@Thickness 0.126 in
Transverse
Linear Mold Shrinkage, Flow 0.014 cm/cm
@Thickness 3.20 mm
0.014 in/in
@Thickness 0.126 in
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break  60.0 MPa
@Temperature 23.0 °C
8700 psi
@Temperature 73.4 °F
ASTM D638
 62.0 MPa
@Temperature 23.0 °C
8990 psi
@Temperature 73.4 °F
ISO 527
Elongation at Break  5.0 %
@Temperature 23.0 °C
5.0 %
@Temperature 73.4 °F
ASTM D638
 5.0 %
@Temperature 23.0 °C
5.0 %
@Temperature 73.4 °F
ISO 527
Tensile Modulus 3.40 GPa
@Temperature 23.0 °C
493 ksi
@Temperature 73.4 °F
ISO 527
Flexural Modulus  3.10 GPa
@Temperature 23.0 °C
450 ksi
@Temperature 73.4 °F
ISO 178
 3.20 GPa
@Temperature 23.0 °C
464 ksi
@Temperature 73.4 °F
ASTM D790
Izod Impact, Notched 1.50 J/cm
@Temperature 23.0 °C
2.81 ft-lb/in
@Temperature 73.4 °F
ASTM D256
Izod Impact, Notched (ISO) 9.00 kJ/m²
@Temperature 23.0 °C
4.28 ft-lb/in²
@Temperature 73.4 °F
ISO 180/1A
Izod Impact, Unnotched (ISO) 45.0 kJ/m²
@Temperature 23.0 °C
21.4 ft-lb/in²
@Temperature 73.4 °F
ISO 180/1U
Charpy Impact Unnotched 5.50 J/cm²
@Temperature 23.0 °C
26.2 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched 0.900 J/cm²
@Temperature 23.0 °C
4.28 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Melting Point 223 °C433 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi) 120 °C248 °FISO 75-1/-2
UL RTI, Electrical  130 °C
@Thickness 0.800 mm
266 °F
@Thickness 0.0315 in
UL 746B
 130 °C
@Thickness 1.50 mm
266 °F
@Thickness 0.0591 in
UL 746B
 130 °C
@Thickness 3.00 mm
266 °F
@Thickness 0.118 in
UL 746B
UL RTI, Mechanical with Impact  130 °C
@Thickness 0.800 mm
266 °F
@Thickness 0.0315 in
UL 746B
 130 °C
@Thickness 1.50 mm
266 °F
@Thickness 0.0591 in
UL 746B
 130 °C
@Thickness 3.00 mm
266 °F
@Thickness 0.118 in
UL 746B
UL RTI, Mechanical without Impact  130 °C
@Thickness 0.800 mm
266 °F
@Thickness 0.0315 in
UL 746B
 130 °C
@Thickness 1.50 mm
266 °F
@Thickness 0.0591 in
UL 746B
 130 °C
@Thickness 3.00 mm
266 °F
@Thickness 0.118 in
UL 746B
Flammability, UL94  V-0
@Thickness 0.800 mm
V-0
@Thickness 0.0315 in
IEC 60695-11-10
 V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
IEC 60695-11-10
 V-0
@Thickness 3.00 mm
V-0
@Thickness 0.118 in
IEC 60695-11-10
 V-0
@Thickness 3.00 mm
V-0
@Thickness 0.118 in
UL94
 V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
UL94
 V-0
@Thickness 0.800 mm
V-0
@Thickness 0.0315 in
UL94
 
Processing PropertiesMetricEnglishComments
Melt Temperature 250 °C482 °FOptimum
 240 - 260 °C464 - 500 °F
Mold Temperature 80.0 °C176 °Foptimum
 30.0 - 130 °C86.0 - 266 °F
Drying Temperature 110 - 130 °C230 - 266 °F
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hour
Moisture Content <= 0.040 %<= 0.040 %
 
Descriptive Properties
AppearanceNatural Color
Drying RecommendedYes
FillerGlass fiber reinforcement
GenericPBT
Material StatusCurrent
Part Marking Code>PBT-IGF5FR(17)<ISO 11469
Polymer FamilyPolyester
Polymer TypePBT
Product CategoryFlame Retardant Resins
 Glass Reinforced Resins
 Toughened Resins
 UV Resistant/Weatherable Resins
Resin IdentificationPBT-IGF5FR(17)ISO 1043

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Zytel® ST801AW NC010 PA66-HI
Polyram PlusTek RB703 Nylon 6, UV Stabilized
Celanese Zytel® 105F BK010 PA66
Celanese Zytel® ST801AW BK195 PA66-HI
Celanese Crastin® SK608 BK509 PBT-GF45

PZDSZ1079 / 139896

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.