MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Overview of materials for Polybutylene Terephthalate (PBT), Unreinforced, Molded
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Unreinforced, Molded

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polybutylene Terephthalate (PBT), Unreinforced, Molded". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 0.900 - 1.92 g/ccAverage value: 1.38 g/cc Grade Count:400
Filler Content 17.0 - 25.0 %Average value: 19.7 % Grade Count:3
Water Absorption 0.000 - 0.600 %Average value: 0.187 % Grade Count:136
Moisture Absorption at Equilibrium 0.0100 - 0.500 %Average value: 0.0970 % Grade Count:171
Water Absorption at Saturation 0.0900 - 0.500 %Average value: 0.380 % Grade Count:64
Viscosity 1.60 - 600000 cPAverage value: 201000 cP Grade Count:7
 7.00 - 87.0 cP
@Temperature 250 - 285 °C
Average value: 36800 cP Grade Count:35
 7.00 - 87.0 cP
@Load 1.20 - 5.00 kg
Average value: 36800 cP Grade Count:35
 8000 - 800000 cP
@Shear Rate 1.00 - 100000 1/s
Average value: 36800 cP Grade Count:2
 8000 - 800000 cP
@Temperature 230 - 270 °C
Average value: 36800 cP Grade Count:2
Viscosity Test 66.5 - 160 cm³/gAverage value: 111 cm³/g Grade Count:20
Viscosity Number 0.600 - 180 cm³/gAverage value: 113 cm³/g Grade Count:17
Maximum Moisture Content 0.0200Average value: 0.0200 Grade Count:25
 0.200 - 0.200
@Temperature 120 - 120 °C
Average value: 0.200 Grade Count:1
 0.200 - 0.200
@Time 299 - 299 sec
Average value: 0.200 Grade Count:1
Linear Mold Shrinkage 0.00100 - 0.0400 cm/cmAverage value: 0.0143 cm/cm Grade Count:313
 0.00400 - 0.0150 cm/cm
@Temperature 80.0 - 80.0 °C
Average value: 0.0136 cm/cm Grade Count:3
 0.0180 - 0.0180 cm/cm
@Temperature 260 - 260 °C
Average value: 0.0136 cm/cm Grade Count:2
 0.0180 - 0.0180 cm/cm
@Pressure 60.0 - 60.0 MPa
Average value: 0.0136 cm/cm Grade Count:2
Linear Mold Shrinkage, Transverse 0.00160 - 0.0400 cm/cmAverage value: 0.0161 cm/cm Grade Count:180
 0.00900 - 0.0170 cm/cm
@Temperature 80.0 - 80.0 °C
Average value: 0.0153 cm/cm Grade Count:3
 0.0180 - 0.0180 cm/cm
@Temperature 260 - 260 °C
Average value: 0.0153 cm/cm Grade Count:2
 0.0180 - 0.0180 cm/cm
@Pressure 60.0 - 60.0 MPa
Average value: 0.0153 cm/cm Grade Count:2
Melt Flow 3.00 - 570 g/10 minAverage value: 38.9 g/10 min Grade Count:191
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 55.0 - 90.0Average value: 80.5 Grade Count:50
Hardness, Rockwell R 107 - 120Average value: 117 Grade Count:25
Hardness, Shore D 40.0 - 87.0Average value: 74.3 Grade Count:24
Ball Indentation Hardness 50.0 - 160 MPaAverage value: 132 MPa Grade Count:21
Tensile Strength, Ultimate 26.0 - 178 MPaAverage value: 74.3 MPa Grade Count:235
Tensile Strength, Yield 21.0 - 166 MPaAverage value: 65.1 MPa Grade Count:231
 22.0 - 105 MPa
@Temperature -40.0 - 100 °C
Average value: 63.5 MPa Grade Count:1
Elongation at Break 0.600 - 300 %Average value: 42.7 % Grade Count:353
 >= 100 %
@Temperature 60.0 - 120 °C
Average value: 100 % Grade Count:2
Elongation at Yield 1.00 - 75.0 %Average value: 6.94 % Grade Count:179
Modulus of Elasticity 0.420 - 23.4 GPaAverage value: 5.18 GPa Grade Count:252
 0.180 - 0.900 GPa
@Temperature 60.0 - 120 °C
Average value: 0.505 GPa Grade Count:2
Flexural Yield Strength 22.0 - 275 MPaAverage value: 112 MPa Grade Count:315
 14.0 - 127 MPa
@Temperature 60.0 - 150 °C
Average value: 60.8 MPa Grade Count:3
Flexural Modulus 0.231 - 18.1 GPaAverage value: 4.50 GPa Grade Count:311
 0.500 - 5.80 GPa
@Temperature 60.0 - 150 °C
Average value: 2.65 GPa Grade Count:3
Flexural Strain at Break 2.00 - 6.00 %Average value: 5.06 % Grade Count:18
 4.60 - 7.00 %
@Temperature 60.0 - 150 °C
Average value: 5.84 % Grade Count:2
Flexural Strain at Yield 5.00 - 8.90 %Average value: 7.00 % Grade Count:22
Adhesive Bond Strength 31.0 - 42.0 MPaAverage value: 36.0 MPa Grade Count:10
Izod Impact 5.00 - 186 JAverage value: 74.4 J Grade Count:77
 30.0 - 144 J
@Temperature -30.0 - -20.0 °C
Average value: 83.1 J Grade Count:25
Izod Impact, Notched 0.0400 - 8.00 J/cmAverage value: 1.02 J/cm Grade Count:115
 0.300 - 0.300 J/cm
@Temperature -20.0 - -20.0 °C
Average value: 2.99 J/cm Grade Count:1
 1.30 - 5.70 J/cm
@Temperature -40.0 - -20.0 °C
Average value: 2.99 J/cm Grade Count:5
 1.30 - 5.70 J/cm
@Thickness 1.57 - 3.18 mm
Average value: 2.99 J/cm Grade Count:5
Izod Impact, Unnotched 0.374 - 5340 J/cmAverage value: 7.29 J/cm Grade Count:85
 5.25 - 6.00 J/cm
@Temperature -30.0 - -30.0 °C
Average value: 5.81 J/cm Grade Count:4
Izod Impact, Notched (ISO) 1.98 - 170 kJ/m²Average value: 11.4 kJ/m² Grade Count:144
 2.00 - 20.0 kJ/m²
@Temperature -40.0 - -20.0 °C
Average value: 9.04 kJ/m² Grade Count:54
Izod Impact, Unnotched (ISO) 4.20 kJ/m² - NBAverage value: 48.8 kJ/m² Grade Count:102
 3.80 kJ/m² - NB
@Temperature -40.0 - -30.0 °C
Average value: 88.9 kJ/m² Grade Count:27
Charpy Impact Unnotched 0.294 J/cm² - NBAverage value: 13.2 J/cm² Grade Count:144
 2.50 J/cm² - NB
@Temperature -40.0 - -20.0 °C
Average value: 14.2 J/cm² Grade Count:89
Charpy Impact, Notched 0.120 J/cm² - NBAverage value: 1.01 J/cm² Grade Count:188
 0.200 - 2.50 J/cm²
@Temperature -40.0 - -20.0 °C
Average value: 0.746 J/cm² Grade Count:95
Gardner Impact 0.904 - 40.0 JAverage value: 28.8 J Grade Count:8
Tensile Impact Strength 65.0 - 160 kJ/m²Average value: 112 kJ/m² Grade Count:3
Dart Drop, Total Energy 2.00 - 140 JAverage value: 21.2 J Grade Count:48
Puncture Energy 15.0 - 16.0 J
@Temperature -30.0 - -30.0 °C
Average value: 15.5 J Grade Count:2
Coefficient of Friction 0.130 - 0.660Average value: 0.346 Grade Count:28
Coefficient of Friction, Static 0.130 - 0.730Average value: 0.362 Grade Count:25
Tensile Creep Modulus, 1 hour 1500 - 2400 MPaAverage value: 2020 MPa Grade Count:6
Tensile Creep Modulus, 1000 hours 950 - 11000 MPaAverage value: 2000 MPa Grade Count:12
K (wear) Factor 4.03 - 423 x 10-8 mm³/N-MAverage value: 114 x 10-8 mm³/N-M Grade Count:24
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 1000 - 1.20e+17 ohm-cmAverage value: 1.61e+16 ohm-cm Grade Count:176
Surface Resistance 10.0 - 2.00e+17 ohmAverage value: 5.58e+15 ohm Grade Count:136
Dielectric Constant 2.90 - 4.20Average value: 3.39 Grade Count:147
Dielectric Strength 14.0 - 140 kV/mmAverage value: 23.7 kV/mm Grade Count:144
Dissipation Factor 0.00100 - 0.0330Average value: 0.0112 Grade Count:135
Arc Resistance 60.0 - 240 secAverage value: 132 sec Grade Count:48
Comparative Tracking Index 120 - 600 VAverage value: 538 V Grade Count:113
Hot Wire Ignition, HWI 7.00 - 120 secAverage value: 52.5 sec Grade Count:12
High Amp Arc Ignition, HAI 15.0 - 120 arcsAverage value: 102 arcs Grade Count:12
High Voltage Arc-Tracking Rate, HVTR 0.000 - 25.4 mm/minAverage value: 12.3 mm/min Grade Count:7
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.0 - 170 µm/m-°CAverage value: 76.8 µm/m-°C Grade Count:231
 25.2 - 171 µm/m-°C
@Temperature 22.8 - 150 °C
Average value: 139 µm/m-°C Grade Count:18
CTE, linear, Transverse to Flow 36.0 - 150 µm/m-°CAverage value: 96.8 µm/m-°C Grade Count:160
 90.0 - 170 µm/m-°C
@Temperature 22.8 - 150 °C
Average value: 151 µm/m-°C Grade Count:14
Specific Heat Capacity 1.50 - 1.97 J/g-°CAverage value: 1.66 J/g-°C Grade Count:7
Thermal Conductivity 0.131 - 0.330 W/m-KAverage value: 0.236 W/m-K Grade Count:13
Melting Point 200 - 271 °CAverage value: 224 °C Grade Count:164
Maximum Service Temperature, Air 60.0 - 200 °CAverage value: 142 °C Grade Count:16
Hot Ball Pressure Test 125 - 200 °CAverage value: 150 °C Grade Count:13
Deflection Temperature at 0.46 MPa (66 psi) 55.0 - 387 °CAverage value: 165 °C Grade Count:284
Deflection Temperature at 1.8 MPa (264 psi) 45.0 - 216 °CAverage value: 100 °C Grade Count:362
Deflection Temperature at 8.0 MPa 45.0 - 48.0 °CAverage value: 45.8 °C Grade Count:4
Vicat Softening Point 65.0 - 221 °CAverage value: 189 °C Grade Count:104
Glass Transition Temp, Tg 60.0 °CAverage value: 60.0 °C Grade Count:15
UL RTI, Electrical 75.0 - 150 °CAverage value: 100 °C Grade Count:45
UL RTI, Mechanical with Impact 75.0 - 140 °CAverage value: 94.3 °C Grade Count:45
UL RTI, Mechanical without Impact 75.0 - 150 °CAverage value: 101 °C Grade Count:45
Flammability, UL94 HB - 5VAGrade Count:261
Oxygen Index 20.0 - 32.0 %Average value: 24.3 % Grade Count:24
Glow Wire Test 650 - 960 °CAverage value: 819 °C Grade Count:45
 
Optical PropertiesOriginal ValueComments
Transmission, Visible 0.600 - 90.0 %Average value: 67.7 % Grade Count:4
 
Processing PropertiesOriginal ValueComments
Processing Temperature 20.0 - 300 °CAverage value: 192 °C Grade Count:52
Nozzle Temperature 225 - 295 °CAverage value: 251 °C Grade Count:104
Adapter Temperature 225 - 275 °CAverage value: 247 °C Grade Count:3
Die Temperature 215 - 275 °CAverage value: 249 °C Grade Count:4
Melt Temperature 174 - 295 °CAverage value: 251 °C Grade Count:223
Mold Temperature 10.0 - 160 °CAverage value: 78.7 °C Grade Count:242
Drying Temperature 80.0 - 150 °CAverage value: 117 °C Grade Count:199
Moisture Content 0.000 - 0.250 %Average value: 0.0493 % Grade Count:42
Dew Point -28.9 °CAverage value: -28.9 °C Grade Count:3
Injection Pressure 3.45 - 120 MPaAverage value: 66.8 MPa Grade Count:37
Vent Depth 0.00127 - 0.00381 cmAverage value: 0.00233 cm Grade Count:16
Precipitation Temperature 40.0 - 270 °CAverage value: 61.3 °C Grade Count:19

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Polyethylene Terephthalate (PET), Unreinforced
Overview of materials for Polyetheretherketone, Unreinforced
Overview of materials for Nylon 6, Unreinforced
Overview of materials for Nylon 66, Unreinforced
Overview of materials for Polyetherimide (PEI)

O3200 / 78165

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.