Applications include low-strength fasteners, die pins, motor spindles, and recessed-head screws. Post water quenched hardness: 41 HRC surface, 95 HRB half-radius, 92 HRB center. Normalized at 925°C in 32 mm rounds, machined to 25 mm, pseudocarburized at 925 for 8 hours, box cooled to RT reheated to 775°C, oil quenched, 150°C temper. |
UNS G10220, AMS 5070, ASTM A29, ASTM A510, ASTM A519, ASTM A544, ASTM A545, ASTM A548, ASTM A576, MIL SPEC MIL-S-11310 (CS1022), SAE J403, SAE J412, SAE J414, DIN 1.1133, UNI G 22 Mn 3, JIS SMnC 21 |