MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Morgan Advanced Ceramics MAFTEC Blanket
Categories: Ceramic; Oxide

Material Notes: MAFTEC Blanket is made from pure mullite fiber only, needled on both sides, and contains no binder or other added constituent. It can be used at continuous operating temperatures up to 1600°C, under oxidizing, neutral or slightly gas-rich conditions, retaining its original toughness, strength and soft, fibrous structure after extended use at this temperature. MAFTEC Blanket is more resistant to acid and alkaline solutions than conventional alumino-silicate fiber blankets. Being virtually free of shot, it has exceptionally good thermal insulation characteristics.

Applications::

  • Furnace and kiln lining (heat treatment, ceramic fast firing, petroleum and chemical)
  • High temperature gaskets
  • Furnace door seals
  • High temperature filter media

Information provided by Morgan Advanced Materials

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.0960 - 0.128 g/cc
@Temperature 23.0 °C
0.00347 - 0.00462 lb/in³
@Temperature 73.4 °F
50% RH
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 0.0930 - 0.103 MPa13.5 - 14.9 psiat 23°C, 50% RH
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity  0.0800 W/m-K
@Temperature 400 °C
0.555 BTU-in/hr-ft²-°F
@Temperature 752 °F
at 96 kg/m3; NFB-40-456
 0.0800 W/m-K
@Temperature 400 °C
0.555 BTU-in/hr-ft²-°F
@Temperature 752 °F
at 128kg/m3; NFB-40-456
 0.0900 W/m-K
@Temperature 500 °C
0.625 BTU-in/hr-ft²-°F
@Temperature 932 °F
at 128kg/m3; NFB-40-456
 0.100 W/m-K
@Temperature 500 °C
0.694 BTU-in/hr-ft²-°F
@Temperature 932 °F
at 96 kg/m3; NFB-40-456
 0.120 W/m-K
@Temperature 600 °C
0.833 BTU-in/hr-ft²-°F
@Temperature 1110 °F
at 128kg/m3; NFB-40-456
 0.130 W/m-K
@Temperature 600 °C
0.902 BTU-in/hr-ft²-°F
@Temperature 1110 °F
at 96 kg/m3; NFB-40-456
 0.140 W/m-K
@Temperature 700 °C
0.972 BTU-in/hr-ft²-°F
@Temperature 1290 °F
at 128kg/m3; NFB-40-456
 0.170 W/m-K
@Temperature 800 °C
1.18 BTU-in/hr-ft²-°F
@Temperature 1470 °F
at 128kg/m3; NFB-40-456
 0.170 W/m-K
@Temperature 700 °C
1.18 BTU-in/hr-ft²-°F
@Temperature 1290 °F
at 96 kg/m3; NFB-40-456
 0.190 W/m-K
@Temperature 800 °C
1.32 BTU-in/hr-ft²-°F
@Temperature 1470 °F
at 96 kg/m3; NFB-40-456
 0.200 W/m-K
@Temperature 900 °C
1.39 BTU-in/hr-ft²-°F
@Temperature 1650 °F
at 128kg/m3; NFB-40-456
 0.230 W/m-K
@Temperature 900 °C
1.60 BTU-in/hr-ft²-°F
@Temperature 1650 °F
at 96 kg/m3; NFB-40-456
 0.240 W/m-K
@Temperature 1000 °C
1.67 BTU-in/hr-ft²-°F
@Temperature 1830 °F
at 128kg/m3; NFB-40-456
 0.270 W/m-K
@Temperature 1000 °C
1.87 BTU-in/hr-ft²-°F
@Temperature 1830 °F
at 96 kg/m3; NFB-40-456
 0.330 W/m-K
@Temperature 1200 °C
2.29 BTU-in/hr-ft²-°F
@Temperature 2190 °F
at 128kg/m3; NFB-40-456
 0.390 W/m-K
@Temperature 1200 °C
2.71 BTU-in/hr-ft²-°F
@Temperature 2190 °F
at 96 kg/m3; NFB-40-456
 0.480 W/m-K
@Temperature 1400 °C
3.33 BTU-in/hr-ft²-°F
@Temperature 2550 °F
at 128kg/m3; NFB-40-456
 0.580 W/m-K
@Temperature 1400 °C
4.03 BTU-in/hr-ft²-°F
@Temperature 2550 °F
at 96 kg/m3; NFB-40-456
Maximum Service Temperature, Air 1600 °C2910 °FContinuous Use
Shrinkage  0.30 %
@Temperature 1300 °C,
Time 86400 sec
0.30 %
@Temperature 2370 °F,
Time 24.0 hour
isothermal
 0.80 %
@Temperature 1400 °C,
Time 86400 sec
0.80 %
@Temperature 2550 °F,
Time 24.0 hour
isothermal
 0.90 %
@Temperature 1500 °C,
Time 86400 sec
0.90 %
@Temperature 2730 °F,
Time 24.0 hour
isothermal
 1.0 %
@Temperature 1600 °C,
Time 86400 sec
1.0 %
@Temperature 2910 °F,
Time 24.0 hour
isothermal
 
Component Elements PropertiesMetricEnglishComments
Al2O3 72 %72 %
Fe2O3 0.030 %0.030 %
K2O+Na2O 0.060 %0.060 %
SiO2 28 %28 %
TiO2 0.010 %0.010 %
 
Descriptive Properties
Colorwhite

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Morgan Advanced Ceramics Cerablanket™ Thermal Ceramic
Morgan Advanced Ceramics Ceramic Fiber Board S Board Ceramic Fibre Board
Morgan Advanced Ceramics Kaowool Ceramic Felt 1260 Thermal Ceramic
Morgan Advanced Ceramics Kaowool HD Organic RCF Vacuum Formed Thermal Ceramic
Morgan Advanced Ceramics Kaowool PM Organic RCF Vacuum Formed Thermal Ceramic

CMORF70128 / 203426

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.