Physical Properties | Metric | English | Comments |
---|
Density | 7.858 g/cc | 0.2839 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Brinell | 111 | 111 |
Hardness, Knoop | 129 | 129 |
Hardness, Rockwell B | 64 | 64 |
Hardness, Vickers | 115 | 115 |
Tensile Strength, Ultimate | 380 MPa | 55100 psi |
Tensile Strength, Yield | 310 MPa | 45000 psi |
Elongation at Break | 15 % | 15 % |
Reduction of Area | 35 % | 35 % |
Modulus of Elasticity | 200 GPa | 29000 ksi |
Bulk Modulus | 160 GPa | 23200 ksi |
Poissons Ratio | 0.29 | 0.29 |
Shear Modulus | 80.0 GPa | 11600 ksi |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.0000159 ohm-cm @Temperature 0.000 °C | 0.0000159 ohm-cm @Temperature 32.0 °F |
| 0.0000219 ohm-cm @Temperature 100 °C | 0.0000219 ohm-cm @Temperature 212 °F |
| 0.0000292 ohm-cm @Temperature 200 °C | 0.0000292 ohm-cm @Temperature 392 °F |
| 0.0000487 ohm-cm @Temperature 400 °C | 0.0000487 ohm-cm @Temperature 752 °F |
| 0.0000758 ohm-cm @Temperature 600 °C | 0.0000758 ohm-cm @Temperature 1110 °F |
| 0.0000925 ohm-cm @Temperature 700 °C | 0.0000925 ohm-cm @Temperature 1290 °F |
| 0.0001094 ohm-cm @Temperature 800 °C | 0.0001094 ohm-cm @Temperature 1470 °F |
| 0.0001136 ohm-cm @Temperature 900 °C | 0.0001136 ohm-cm @Temperature 1650 °F |
| 0.0001167 ohm-cm @Temperature 1000 °C | 0.0001167 ohm-cm @Temperature 1830 °F |
| 0.0001194 ohm-cm @Temperature 1100 °C | 0.0001194 ohm-cm @Temperature 2010 °F |
| 0.0001219 ohm-cm @Temperature 1200 °C | 0.0001219 ohm-cm @Temperature 2190 °F |
| 0.0001239 ohm-cm @Temperature 1300 °C | 0.0001239 ohm-cm @Temperature 2370 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 12.1 µm/m-°C @Temperature 20.0 - 100 °C | 6.72 µin/in-°F @Temperature 68.0 - 212 °F |
| 12.8 µm/m-°C @Temperature 20.0 - 200 °C | 7.11 µin/in-°F @Temperature 68.0 - 392 °F |
| 13.3 µm/m-°C @Temperature 20.0 - 300 °C | 7.39 µin/in-°F @Temperature 68.0 - 572 °F |
| 13.9 µm/m-°C @Temperature 20.0 - 400 °C | 7.72 µin/in-°F @Temperature 68.0 - 752 °F |
| 14.4 µm/m-°C @Temperature 20.0 - 500 °C | 8.00 µin/in-°F @Temperature 68.0 - 932 °F |
| 14.8 µm/m-°C @Temperature 20.0 - 600 °C | 8.22 µin/in-°F @Temperature 68.0 - 1110 °F |
Specific Heat Capacity | 0.486 J/g-°C @Temperature >=100 °C | 0.116 BTU/lb-°F @Temperature >=212 °F |
| 0.519 J/g-°C @Temperature 150 - 200 °C | 0.124 BTU/lb-°F @Temperature 302 - 392 °F |
| 0.532 J/g-°C @Temperature 200 - 250 °C | 0.127 BTU/lb-°F @Temperature 392 - 482 °F |
| 0.557 J/g-°C @Temperature 250 - 300 °C | 0.133 BTU/lb-°F @Temperature 482 - 572 °F |
| 0.574 J/g-°C @Temperature 300 - 350 °C | 0.137 BTU/lb-°F @Temperature 572 - 662 °F |
| 0.599 J/g-°C @Temperature 350 - 400 °C | 0.143 BTU/lb-°F @Temperature 662 - 752 °F |
| 0.662 J/g-°C @Temperature 450 - 500 °C | 0.158 BTU/lb-°F @Temperature 842 - 932 °F |
| 0.749 J/g-°C @Temperature 550 - 600 °C | 0.179 BTU/lb-°F @Temperature 1020 - 1110 °F |
| 0.846 J/g-°C @Temperature 650 - 700 °C | 0.202 BTU/lb-°F @Temperature 1200 - 1290 °F |
| 0.950 J/g-°C @Temperature 750 - 800 °C | 0.227 BTU/lb-°F @Temperature 1380 - 1470 °F |
| 1.432 J/g-°C @Temperature 700 - 750 °C | 0.3423 BTU/lb-°F @Temperature 1290 - 1380 °F |
Thermal Conductivity | 26.1 W/m-K @Temperature 800 °C | 181 BTU-in/hr-ft²-°F @Temperature 1470 °F |
| 31.8 W/m-K @Temperature 700 °C | 221 BTU-in/hr-ft²-°F @Temperature 1290 °F |
| 35.6 W/m-K @Temperature 600 °C | 247 BTU-in/hr-ft²-°F @Temperature 1110 °F |
| 39.4 W/m-K @Temperature 500 °C | 273 BTU-in/hr-ft²-°F @Temperature 932 °F |
| 42.7 W/m-K @Temperature 400 °C | 296 BTU-in/hr-ft²-°F @Temperature 752 °F |
| 46.0 W/m-K @Temperature 300 °C | 319 BTU-in/hr-ft²-°F @Temperature 572 °F |
| 49.0 W/m-K @Temperature 200 °C | 340 BTU-in/hr-ft²-°F @Temperature 392 °F |
| 51.2 W/m-K @Temperature 100 °C | 355 BTU-in/hr-ft²-°F @Temperature 212 °F |
| 51.9 W/m-K @Temperature 0.000 °C | 360 BTU-in/hr-ft²-°F @Temperature 32.0 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Carbon, C | 0.22 - 0.28 % | 0.22 - 0.28 % |
Iron, Fe | 99.03 - 99.48 % | 99.03 - 99.48 % |
Manganese, Mn | 0.30 - 0.60 % | 0.30 - 0.60 % |
Phosphorus, P | <= 0.040 % | <= 0.040 % |
Sulfur, S | <= 0.050 % | <= 0.050 % |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view