Physical Properties | Metric | English | Comments |
---|
Density | 8.14 g/cc | 0.294 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength at Break | 173 MPa @Temperature 1000 °C | 25100 psi @Temperature 1830 °F |
| 180 MPa @Temperature 1093 °C | 26100 psi @Temperature 1999 °F |
| 190 MPa @Temperature 1093 °C | 27600 psi @Temperature 1999 °F |
| 240 MPa @Temperature 982 °C | 34800 psi @Temperature 1800 °F |
| 250 MPa @Temperature 982 °C | 36300 psi @Temperature 1800 °F |
| 546 MPa @Temperature 700 °C | 79200 psi @Temperature 1290 °F |
| 853 MPa @Temperature 200 °C | 124000 psi @Temperature 392 °F |
| 949 MPa @Temperature 20.0 °C | 138000 psi @Temperature 68.0 °F |
| 960 MPa @Temperature 20.0 °C | 139000 psi @Temperature 68.0 °F |
| 1030 MPa @Temperature 20.0 °C | 149000 psi @Temperature 68.0 °F |
Tensile Strength, Yield | 151 MPa @Strain 0.2 %, Temperature 1000 °C | 21900 psi @Strain 0.2 %, Temperature 1830 °F |
| 160 MPa @Strain 0.2 %, Temperature 1093 °C | 23200 psi @Strain 0.2 %, Temperature 1999 °F |
| 170 MPa @Strain 0.2 %, Temperature 1093 °C | 24700 psi @Strain 0.2 %, Temperature 1999 °F |
| 220 MPa @Strain 0.2 %, Temperature 982 °C | 31900 psi @Strain 0.2 %, Temperature 1800 °F |
| 220 MPa @Strain 0.2 %, Temperature 982 °C | 31900 psi @Strain 0.2 %, Temperature 1800 °F |
| 371 MPa @Strain 0.2 %, Temperature 700 °C | 53800 psi @Strain 0.2 %, Temperature 1290 °F |
| 495 MPa @Strain 0.2 %, Temperature 200 °C | 71800 psi @Strain 0.2 %, Temperature 392 °F |
| 560 MPa @Strain 0.2 %, Temperature 20.0 °C | 81200 psi @Strain 0.2 %, Temperature 68.0 °F |
| 680 MPa @Strain 0.2 %, Temperature 20.0 °C | 98600 psi @Strain 0.2 %, Temperature 68.0 °F |
| 690 MPa @Strain 0.2 %, Temperature 20.0 °C | 100000 psi @Strain 0.2 %, Temperature 68.0 °F |
Elongation at Break | 4.0 % @Temperature 1093 °C | 4.0 % @Temperature 1999 °F |
| 4.0 % @Temperature 982 °C | 4.0 % @Temperature 1800 °F |
| 5.0 % @Temperature 1093 °C | 5.0 % @Temperature 1999 °F |
| 6.0 % @Temperature 982 °C | 6.0 % @Temperature 1800 °F |
| 14 % @Temperature 20.0 °C | 14 % @Temperature 68.0 °F |
| 22 % @Temperature 20.0 °C | 22 % @Temperature 68.0 °F |
| 22 % @Temperature 200 °C | 22 % @Temperature 392 °F |
| 27 % @Temperature 20.0 °C | 27 % @Temperature 68.0 °F |
| 29 % @Temperature 700 °C | 29 % @Temperature 1290 °F |
| 29 % @Temperature 1000 °C | 29 % @Temperature 1830 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.0001137 ohm-cm @Temperature 22.0 °C | 0.0001137 ohm-cm @Temperature 71.6 °F |
| 0.000115 ohm-cm @Temperature 93.0 °C | 0.000115 ohm-cm @Temperature 199 °F |
| 0.0001203 ohm-cm @Temperature 538 °C | 0.0001203 ohm-cm @Temperature 1000 °F |
| 0.0001204 ohm-cm @Temperature 982 °C | 0.0001204 ohm-cm @Temperature 1800 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 12.47 µm/m-°C @Temperature 200 °C | 6.928 µin/in-°F @Temperature 392 °F |
| 13.39 µm/m-°C @Temperature 600 °C | 7.439 µin/in-°F @Temperature 1110 °F |
| 14.24 µm/m-°C @Temperature 1000 °C | 7.911 µin/in-°F @Temperature 1830 °F |
| 15.03 µm/m-°C @Temperature 1400 °C | 8.350 µin/in-°F @Temperature 2550 °F |
Melting Point | 1375 °C | 2507 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Aluminum, Al | 0.30 % | 0.30 % |
Carbon, C | 0.050 % | 0.050 % |
Chromium, Cr | 30 % | 30 % |
Iron, Fe | 1.0 % | 1.0 % |
Nickel, Ni | 67.55 % | 67.55 % |
Titanium, Ti | 0.50 % | 0.50 % |
Y2O3 | 0.60 % | 0.60 % |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.