MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Victrex APTIV™ 1102-050M Polyetheretherketone (PEEK) Polymer Film, Semi-Crystalline, 20% Mineral Filled
Categories: Polymer; Film; Thermoplastic; Polyketone; Polyetheretherketone (PEEK)

Material Notes: APTIV™ PEEK 1100 series films are the mineral filled semi-crystalline films made from VICTREX™ PEEK polymer. The film provides a material solution for engineers in ultra-high performance applications.

APTIV PEEK 1100 has a unique combination of properties providing high temperature performance, mechanical strength, durability, excellent radiation, hydrolysis and chemical resistance, electrical insulation, excellent barrier properties with high purity, good flammability without the use of flame retardants, low toxicity of combustion products, and low moisture absorption in a film format. Inherently halogen free and ease of processing makes APTIV films a technology enabler for our customers and end users. APTIV PEEK 1100 series provides a higher modulus and lower coefficient of linear thermal expansion over the APTIV 1000 series.

Applications:

  • Electrical Insulation
  • Printed circuit substrates
  • High temperature labels
  • Flexible surface heaters
  • Pressure sensor membranes
  • Acoustic speaker diaphragms and voice coils
  • Proven temperature resistance to use of lead free solders
APTIV film is FDA and EU approved for food contact and is RoHS compliant.

All information provided by Victrex.

Property data reported herein was measured on 50 micron film. The films are available in thicknesses from 12 microns up to 125 microns.

Vendors: Victrex is a global leader in high-performance PEEK and PAEK polymers, transforming industries from aerospace to medical devices. For 40 years, our innovative polymer solutions help customers achieve new levels of performance, sustainability, and cost efficiency across applications that millions rely on daily from smartphones to aircraft components. As pioneers in polymer engineering, we're committed to delivering transformational solutions that address global materials challenges. Visit www.victrex.com, call (800) VICTREX /1-484-342-6001, or email victrexplc@victrex.com.

Ensinger TECAPEEK™ shapes are manufactured exclusively with Victrex™ PEEK polymer. The Ensinger process and Victrex resins ensure reliability, consistency, dimensional stability, and high temperature mechanical performance.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.45 g/cc
@Temperature 23.0 °C
1.45 g/cc
@Temperature 73.4 °F
ISO 1183
Moisture Absorption at Equilibrium 0.080 %
@Temperature 23.0 °C,
Time 86400 sec
0.080 %
@Temperature 73.4 °F,
Time 24.0 hour
50% RH; ISO 62
 
Mechanical PropertiesMetricEnglishComments
Film Elongation at Break, MD >= 100 %>= 100 %ISO 527
 >= 100 %
@Thickness 0.0250 mm
>= 100 %
@Thickness 0.000984 in
ISO 527
 >= 100 %
@Thickness 0.0250 mm
>= 100 %
@Thickness 0.000984 in
ISO 527
Film Elongation at Break, TD >= 10 %>= 10 %ISO 527
 >= 10 %
@Thickness 0.100 mm
>= 10 %
@Thickness 0.00394 in
ISO 527
 >= 10 %
@Thickness 0.100 mm
>= 10 %
@Thickness 0.00394 in
ISO 527
Tensile Modulus 4.30 GPa624 ksiTD; ISO 527
 4.80 GPa696 ksiMD; ISO 527
 4.20 GPa
@Thickness 0.100 mm
609 ksi
@Thickness 0.00394 in
TD; ISO 527
 4.50 GPa
@Thickness 0.0250 mm
653 ksi
@Thickness 0.000984 in
TD; ISO 527
 4.50 GPa
@Thickness 0.100 mm
653 ksi
@Thickness 0.00394 in
MD; ISO 527
 5.00 GPa
@Thickness 0.0250 mm
725 ksi
@Thickness 0.000984 in
MD; ISO 527
Tear Strength 5.96 kN/m34.0 pliMD; ISO 6383-1
 6.84 kN/m39.0 pliTD; ISO 6383-1
Film Tensile Strength at Break, MD 100 MPa14500 psiISO 527
 100 MPa
@Thickness 0.0250 mm
14500 psi
@Thickness 0.000984 in
ISO 527
 100 MPa
@Thickness 0.100 mm
14500 psi
@Thickness 0.00394 in
ISO 527
Film Tensile Strength at Break, TD 80.0 MPa11600 psiISO 527
 80.0 MPa
@Thickness 0.0250 mm
11600 psi
@Thickness 0.000984 in
ISO 527
 80.0 MPa
@Thickness 0.100 mm
11600 psi
@Thickness 0.00394 in
ISO 527
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+16 ohm-cm
@Temperature 23.0 °C
1.00e+16 ohm-cm
@Temperature 73.4 °F
100V; ASTM D257
Dielectric Constant 3.6
@Frequency 1e+7 Hz,
Temperature 23.0 °C
3.6
@Frequency 1e+7 Hz,
Temperature 73.4 °F
Dielectric Strength 200 kV/mm
@Temperature 23.0 °C
5080 kV/in
@Temperature 73.4 °F
1/4 inch electrode; ASTM D149
Dissipation Factor 0.0010
@Frequency 1e+7 Hz,
Temperature 23.0 °C
0.0010
@Frequency 1e+7 Hz,
Temperature 73.4 °F
ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear 35.0 µm/m-°C19.4 µin/in-°FMD, below Tg; ASTM D696
Thermal Conductivity 0.430 W/m-K2.98 BTU-in/hr-ft²-°FThrough Plane; ASTM E1461
 0.910 W/m-K6.32 BTU-in/hr-ft²-°FIn-Plane; ASTM E1461
Shrinkage, MD <= 0.50 %
@Temperature 200 °C
<= 0.50 %
@Temperature 392 °F
TM-XV-84
Shrinkage, TD <= 0.50 %
@Temperature 200 °C
<= 0.50 %
@Temperature 392 °F
TM-XV-84
 
Descriptive Properties
Puncture Strength5 kJ/m²MD/TD, Def Stan 81-75; 23°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Lotte Advanced Materials Infino® FD-1102 PC, FR
ExxonMobil ESCOREZ™ 1102RM (Europe) Petroleum Hydrocarbon Resin
ExxonMobil ESCOREZ™ 1102 (Americas) Petroleum Hydrocarbon Resin
SunChemical Gwent D2121102P1 UV Curable Dielectric Ink
VICTREX™ PEEK 150CA30 30% Carbon Fiber Reinforced

PVICTA47 / 83663

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.