Physical Properties | Metric | English | Comments |
---|
Density | 2.20 g/cc | 0.0795 lb/in³ |
Moisture Absorption at Equilibrium | 0.020 % @Thickness 1.57 mm | 0.020 % @Thickness 0.0620 in |
Thickness | 127 - 3180 microns | 5.00 - 125 mil |
Deformation | 1.0 % @Pressure 14.0 MPa, Temperature 150 °C | 1.0 % @Pressure 2030 psi, Temperature 302 °F |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength, Ultimate | 18.0 MPa @Temperature 100 °C | 2610 psi @Temperature 212 °F |
| 20.0 MPa @Temperature 100 °C | 2900 psi @Temperature 212 °F |
| 27.0 MPa @Temperature 23.0 °C | 3920 psi @Temperature 73.4 °F |
| 29.0 MPa @Temperature 23.0 °C | 4210 psi @Temperature 73.4 °F |
Elongation at Break | 4.9 % @Temperature 23.0 °C | 4.9 % @Temperature 73.4 °F |
| 5.8 % @Temperature 100 °C | 5.8 % @Temperature 212 °F |
| 6.0 % @Temperature 23.0 °C | 6.0 % @Temperature 73.4 °F |
| 7.2 % @Temperature 100 °C | 7.2 % @Temperature 212 °F |
Tensile Modulus | 0.379 GPa @Temperature 100 °C | 55.0 ksi @Temperature 212 °F |
| 0.448 GPa @Temperature 100 °C | 65.0 ksi @Temperature 212 °F |
| 0.862 GPa @Temperature 23.0 °C | 125 ksi @Temperature 73.4 °F |
| 1.08 GPa @Temperature 23.0 °C | 156 ksi @Temperature 73.4 °F |
Compressive Strength | 21.0 MPa @Strain 7.8 %, Temperature 100 °C | 3050 psi @Strain 7.8 %, Temperature 212 °F |
| 22.0 MPa @Strain 8.4 %, Temperature 100 °C | 3190 psi @Strain 8.4 %, Temperature 212 °F |
| 27.0 MPa @Strain 8.5 %, Temperature 23.0 °C | 3920 psi @Strain 8.5 %, Temperature 73.4 °F |
| 29.0 MPa @Strain 7.7 %, Temperature 23.0 °C | 4210 psi @Strain 7.7 %, Temperature 73.4 °F |
| 43.0 MPa @Strain 17.6 %, Temperature 100 °C | 6240 psi @Strain 17.6 %, Temperature 212 °F |
| 52.0 MPa @Strain 12.5 %, Temperature 23.0 °C | 7540 psi @Strain 12.5 %, Temperature 73.4 °F |
Compressive Modulus | 0.500 GPa @Temperature 100 °C | 72.5 ksi @Temperature 212 °F |
| 0.500 GPa @Temperature 100 °C | 72.5 ksi @Temperature 212 °F |
| 0.670 GPa @Temperature 100 °C | 97.2 ksi @Temperature 212 °F |
| 0.710 GPa @Temperature 23.0 °C | 103 ksi @Temperature 73.4 °F |
| 0.710 GPa @Temperature 23.0 °C | 103 ksi @Temperature 73.4 °F |
| 0.940 GPa @Temperature 23.0 °C | 136 ksi @Temperature 73.4 °F |
Peel Strength | 5.47 kN/m | 31.2 pli |
|
Electrical Properties | Metric | English | Comments |
---|
Volume Resistivity | 2.00e+13 ohm-cm | 2.00e+13 ohm-cm |
Surface Resistance | 3.00e+13 ohm | 3.00e+13 ohm |
Dielectric Constant | 2.2 @Frequency 8.00e+9 - 4.00e+10 Hz | 2.2 @Frequency 8.00e+9 - 4.00e+10 Hz |
| 2.18 - 2.24 @Frequency 1e+10 Hz | 2.18 - 2.24 @Frequency 1e+10 Hz |
Dissipation Factor | 0.00040 @Frequency 1e+6 Hz | 0.00040 @Frequency 1e+6 Hz |
| 0.00090 @Frequency 1e+10 Hz | 0.00090 @Frequency 1e+10 Hz |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 31.0 µm/m-°C @Temperature 0.000 - 100 °C | 17.2 µin/in-°F @Temperature 32.0 - 212 °F |
| 48.0 µm/m-°C @Temperature 0.000 - 100 °C | 26.7 µin/in-°F @Temperature 32.0 - 212 °F |
| 237 µm/m-°C @Temperature 0.000 - 100 °C | 132 µin/in-°F @Temperature 32.0 - 212 °F |
Specific Heat Capacity | 0.960 J/g-°C | 0.229 BTU/lb-°F |
Thermal Conductivity | 0.200 W/m-K @Temperature 80.0 °C | 1.39 BTU-in/hr-ft²-°F @Temperature 176 °F |
Deflection Temperature at 1.8 MPa (264 psi) | >= 260 °C | >= 500 °F |
Decomposition Temperature | 500 °C | 932 °F |
Flammability, UL94 | V-0 | V-0 |
|
Descriptive Properties |
---|
Thermal Coefficient of Dielectric Constant | -125 ppm/°C |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.