Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 1.20 g/cc | 1.20 g/cc |
Water Absorption | 0.15 % @Temperature 23.0 °C, Time 86400 sec | 0.15 % @Temperature 73.4 °F, Time 24.0 hour |
Moisture Absorption at Equilibrium | 0.32 % @Temperature 23.0 °C | 0.32 % @Temperature 73.4 °F |
Linear Mold Shrinkage, Flow | 0.00050 - 0.00070 cm/cm | 0.00050 - 0.00070 in/in |
Melt Flow | 3.0 g/10 min @Load 1.20 kg, Temperature 300 °C | 3.0 g/10 min @Load 2.65 lb, Temperature 572 °F |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Rockwell M | 73 | 73 |
Tensile Strength, Ultimate | 66.0 MPa | 9570 psi |
Tensile Strength, Yield | 62.0 MPa | 8990 psi |
Elongation at Break | 120 % | 120 % |
Elongation at Yield | 6.0 % | 6.0 % |
Tensile Modulus | 2.20 GPa | 319 ksi |
Flexural Yield Strength | 90.0 MPa | 13100 psi |
Flexural Modulus | 2.20 GPa | 319 ksi |
Izod Impact, Notched | 9.074 J/cm @Thickness 3.20 mm, Temperature 23.0 °C | 17.00 ft-lb/in @Thickness 0.126 in, Temperature 73.4 °F |
Izod Impact, Unnotched | NB @Temperature 23.0 °C | NB @Temperature 73.4 °F |
Dart Drop, Total Energy | 89.0 J @Thickness 3.20 mm | 65.6 ft-lb @Thickness 0.126 in |
Abrasion | 45 @Load 1.00 kg | 45 @Load 2.20 lb |
|
Electrical Properties | Metric | English | Comments |
---|
Volume Resistivity | 2.00e+17 ohm-cm | 2.00e+17 ohm-cm |
Dielectric Constant | 3.0 @Frequency 60 Hz | 3.0 @Frequency 60 Hz |
Dielectric Strength | 17.0 kV/mm | 432 kV/in |
Dissipation Factor | 0.0010 @Frequency 60.0 Hz | 0.0010 @Frequency 60.0 Hz |
Arc Resistance | 0.00 - 60 sec | 0.00 - 60 sec |
Comparative Tracking Index | 225 V @Thickness 2.00 mm | 225 V @Thickness 0.0787 in |
Hot Wire Ignition, HWI | 15 - 30 sec @Thickness >=1.50 mm | 15 - 30 sec @Thickness >=0.0591 in |
| 15 - 30 sec @Thickness >=2.00 mm | 15 - 30 sec @Thickness >=0.0787 in |
| 30 - 60 sec @Thickness >=3.00 mm | 30 - 60 sec @Thickness >=0.118 in |
High Amp Arc Ignition, HAI | >= 120 arcs @Thickness 1.50 mm | >= 120 arcs @Thickness 0.0591 in |
| >= 120 arcs @Thickness 2.00 mm | >= 120 arcs @Thickness 0.0787 in |
| >= 120 arcs @Thickness 3.00 mm | >= 120 arcs @Thickness 0.118 in |
High Voltage Arc-Tracking Rate, HVTR | 80.0 - 150 mm/min | 3.15 - 5.91 in/min |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 68.0 µm/m-°C @Temperature -40.0 - 82.0 °C | 37.8 µin/in-°F @Temperature -40.0 - 180 °F |
Hot Ball Pressure Test | >= 125 °C | >= 257 °F |
Deflection Temperature at 0.46 MPa (66 psi) | 138 °C @Thickness 4.00 mm | 280 °F @Thickness 0.157 in |
Deflection Temperature at 1.8 MPa (264 psi) | 126 °C @Thickness 4.00 mm | 259 °F @Thickness 0.157 in |
Vicat Softening Point | 147 °C @Load 5.10 kg | 297 °F @Load 11.2 lb |
Softening Point | 150 - 200 °C | 302 - 392 °F |
UL RTI, Electrical | 130 °C @Thickness >=0.750 mm | 266 °F @Thickness >=0.0295 in |
| 130 °C @Thickness >=1.50 mm | 266 °F @Thickness >=0.0591 in |
| 130 °C @Thickness >=2.00 mm | 266 °F @Thickness >=0.0787 in |
| 130 °C @Thickness >=3.00 mm | 266 °F @Thickness >=0.118 in |
UL RTI, Mechanical with Impact | 110 °C @Thickness >=0.750 mm | 230 °F @Thickness >=0.0295 in |
| 110 °C @Thickness >=1.50 mm | 230 °F @Thickness >=0.0591 in |
| 110 °C @Thickness >=2.00 mm | 230 °F @Thickness >=0.0787 in |
| 110 °C @Thickness >=3.00 mm | 230 °F @Thickness >=0.118 in |
UL RTI, Mechanical without Impact | 130 °C @Thickness >=0.750 mm | 266 °F @Thickness >=0.0295 in |
| 130 °C @Thickness >=1.50 mm | 266 °F @Thickness >=0.0591 in |
| 130 °C @Thickness >=2.00 mm | 266 °F @Thickness >=0.0787 in |
| 130 °C @Thickness >=3.00 mm | 266 °F @Thickness >=0.118 in |
Flammability, UL94 | V-0 @Thickness 1.50 mm | V-0 @Thickness 0.0591 in |
| V-0 @Thickness 2.00 mm | V-0 @Thickness 0.0787 in |
| V-0 @Thickness 3.00 mm | V-0 @Thickness 0.118 in |
Flash Point | >= 450 °C | >= 842 °F |
Oxygen Index | 35 % | 35 % |
Glow Wire Test | 960 °C @Thickness 2.00 mm, Time 5.00 sec | 1760 °F @Thickness 0.0787 in, Time 0.00139 hour |
Ignition Temperature | >= 450 °C | >= 842 °F |
|
Optical Properties | Metric | English | Comments |
---|
Refractive Index | 1.586 | 1.586 |
Haze | 0.70 - 2.0 % | 0.70 - 2.0 % |
Transmission, Visible | 89 % | 89 % |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.