MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Special Metals MONEL® Alloy K-500
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: A precipitation-hardenable nickel-copper alloy that combines the corrosion resistance of MONEL alloy 400 with greater strength and hardness. It also has low permeability and is nonmagnetic to under -150°F (-101°C). Used for pump shafts, oil-well tools and instruments, doctor blades and scrapers, springs, valve trim, fasteners, and marine propeller shafts. Standard product forms are round, hexagon, flats, forging stock, pipe, tube, plate, sheet, strip, and wire.

Data provided by the manufacturer, Special Metals.

Key Words: DIN 17743, 17752, 17754; Werkstoff Nr. 2.4375; QQ-N-286; NACE MR -01-75, Monel Nickel-Copper Alloy, UNS N05500; BS 3072 - 3076 (NA18); ASME Boiler Code Section VIII; SAE AMS 4676; MIL-N-24549
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.44 g/cc0.305 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate  860 MPa
@Temperature 425 °C
125000 psi
@Temperature 797 °F
Precipitation Hardened prior to test
 1100 MPa
@Temperature 23.0 °C
160000 psi
@Temperature 73.4 °F
Tensile Strength, Yield 790 MPa
@Strain 0.2 %
115000 psi
@Strain 0.2 %
Precipitation Hardened. Value at room temperature
 630 MPa
@Strain 0.2 %,
Temperature 425 °C
91400 psi
@Strain 0.2 %,
Temperature 797 °F
Precipitation Hardened prior to test
Elongation at Break 25 %25 %Precipitation Hardened
 12 %
@Temperature 425 °C
12 %
@Temperature 797 °F
Precipitation Hardened prior to test.
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000615 ohm-cm0.0000615 ohm-cm
Magnetic Permeability 1.0021.002at 200 Oersted (15.9 kA/m)
Curie Temperature -65.0 °C-85.0 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear 13.7 µm/m-°C
@Temperature 20.0 - 100 °C
7.61 µin/in-°F
@Temperature 68.0 - 212 °F
Specific Heat Capacity 0.419 J/g-°C0.100 BTU/lb-°F
Thermal Conductivity 17.5 W/m-K121 BTU-in/hr-ft²-°F
Melting Point 1315 - 1350 °C2399 - 2460 °F
Solidus 1315 °C2399 °F
Liquidus 1350 °C2460 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 2.3 - 3.15 %2.3 - 3.15 %
Carbon, C <= 0.25 %<= 0.25 %
Copper, Cu 27 - 33 %27 - 33 %
Iron, Fe <= 2.0 %<= 2.0 %
Manganese, Mn <= 1.5 %<= 1.5 %
Nickel, Ni >= 63 %>= 63 %
Silicon, Si <= 0.50 %<= 0.50 %
Sulfur, S <= 0.010 %<= 0.010 %
Titanium, Ti 0.35 - 0.85 %0.35 - 0.85 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Special Metals MONEL® Alloy 400
ATI Allvac® Nickelvac® K-500 UNS N05500 Nickel Superalloy
MetalTek MTEK B Cast UNS N24030 Nickel-Copper Alloy
Special Metals MONEL® Alloy R-405
Special Metals MONEL® Alloy 401

NINC14 / 17397

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.