Physical Properties | Metric | English | Comments |
---|
Density | 7.65 g/cc | 0.276 lb/in³ |
Thickness | 270 - 310 microns | 10.6 - 12.2 mil |
| 300 microns | 11.8 mil |
|
Mechanical Properties | Metric | English | Comments |
---|
Knoop Microhardness | 173 | 173 |
Hardness, Rockwell B | 83 | 83 |
Tensile Strength, Ultimate | 359 MPa | 52100 psi |
Tensile Strength, Yield | 345 MPa | 50000 psi |
Elongation at Break | 11 % | 11 % |
Modulus of Elasticity | 113.8 GPa | 16510 ksi |
| 138 GPa | 20000 ksi |
| 203 GPa | 29400 ksi |
| 241 GPa | 35000 ksi |
| 276 GPa | 40000 ksi |
|
Electrical Properties | Metric | English | Comments |
---|
Exciting Power (RMS) | 0.00171 RMS AT/cm @Magnetic Field 0.100 T, Frequency 50 Hz | 0.00270 RMS VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00215 RMS AT/cm @Magnetic Field 0.100 T, Frequency 60 Hz | 0.00340 RMS VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00601 RMS AT/cm @Magnetic Field 0.200 T, Frequency 50 Hz | 0.00950 RMS VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.00772 RMS AT/cm @Magnetic Field 0.200 T, Frequency 60 Hz | 0.0122 RMS VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0126 RMS AT/cm @Magnetic Field 0.300 T, Frequency 50 Hz | 0.0199 RMS VA/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0163 RMS AT/cm @Magnetic Field 0.300 T, Frequency 60 Hz | 0.0257 RMS VA/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0212 RMS AT/cm @Magnetic Field 0.400 T, Frequency 50 Hz | 0.0335 RMS VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0274 RMS AT/cm @Magnetic Field 0.400 T, Frequency 60 Hz | 0.0433 RMS VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0314 RMS AT/cm @Magnetic Field 0.500 T, Frequency 50 Hz | 0.0496 RMS VA/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0407 RMS AT/cm @Magnetic Field 0.500 T, Frequency 60 Hz | 0.0644 RMS VA/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0433 RMS AT/cm @Magnetic Field 0.600 T, Frequency 50 Hz | 0.0684 RMS VA/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0562 RMS AT/cm @Magnetic Field 0.600 T, Frequency 60 Hz | 0.0888 RMS VA/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.0568 RMS AT/cm @Magnetic Field 0.700 T, Frequency 50 Hz | 0.0897 RMS VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.07219 RMS AT/cm @Magnetic Field 0.800 T, Frequency 50 Hz | 0.1141 RMS VA/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.07390 RMS AT/cm @Magnetic Field 0.700 T, Frequency 60 Hz | 0.1168 RMS VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.08972 RMS AT/cm @Magnetic Field 0.900 T, Frequency 50 Hz | 0.1418 RMS VA/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.09377 RMS AT/cm @Magnetic Field 0.800 T, Frequency 60 Hz | 0.1482 RMS VA/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.1102 RMS AT/cm @Magnetic Field 1.00 T, Frequency 50 Hz | 0.1741 RMS VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.1165 RMS AT/cm @Magnetic Field 0.900 T, Frequency 60 Hz | 0.1841 RMS VA/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.1340 RMS AT/cm @Magnetic Field 1.10 T, Frequency 50 Hz | 0.2118 RMS VA/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.1432 RMS AT/cm @Magnetic Field 1.00 T, Frequency 60 Hz | 0.2264 RMS VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.1619 RMS AT/cm @Magnetic Field 1.20 T, Frequency 50 Hz | 0.2559 RMS VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.174 RMS AT/cm @Magnetic Field 1.10 T, Frequency 60 Hz | 0.275 RMS VA/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.1953 RMS AT/cm @Magnetic Field 1.30 T, Frequency 50 Hz | 0.3086 RMS VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.2099 RMS AT/cm @Magnetic Field 1.20 T, Frequency 60 Hz | 0.3318 RMS VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.2352 RMS AT/cm @Magnetic Field 1.40 T, Frequency 50 Hz | 0.3718 RMS VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.2522 RMS AT/cm @Magnetic Field 1.30 T, Frequency 60 Hz | 0.3986 RMS VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.2856 RMS AT/cm @Magnetic Field 1.50 T, Frequency 50 Hz | 0.4514 RMS VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.3028 RMS AT/cm @Magnetic Field 1.40 T, Frequency 60 Hz | 0.4786 RMS VA/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.3549 RMS AT/cm @Magnetic Field 1.60 T, Frequency 50 Hz | 0.5609 RMS VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.3655 RMS AT/cm @Magnetic Field 1.50 T, Frequency 60 Hz | 0.5777 RMS VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.4504 RMS AT/cm @Magnetic Field 1.60 T, Frequency 60 Hz | 0.7118 RMS VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.4702 RMS AT/cm @Magnetic Field 1.70 T, Frequency 50 Hz | 0.7432 RMS VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.5895 RMS AT/cm @Magnetic Field 1.70 T, Frequency 60 Hz | 0.9318 RMS VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 0.77651 RMS AT/cm @Magnetic Field 1.80 T, Frequency 50 Hz | 1.2273 RMS VA/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 0.95190 RMS AT/cm @Magnetic Field 1.80 T, Frequency 60 Hz | 1.5045 RMS VA/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 2.8414 RMS AT/cm @Magnetic Field 1.90 T, Frequency 50 Hz | 4.4909 RMS VA/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 3.5230 RMS AT/cm @Magnetic Field 1.90 T, Frequency 60 Hz | 5.5682 RMS VA/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
Electrical Resistivity | 0.0000500 ohm-cm | 0.0000500 ohm-cm |
|
Magnetic Properties | Metric | English | Comments |
---|
Core Loss | 0.00361 W/kg @Magnetic Field 0.100 T, Frequency 50 Hz | 0.00164 W/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00487 W/kg @Magnetic Field 0.100 T, Frequency 60 Hz | 0.00221 W/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.01382 W/kg @Magnetic Field 0.200 T, Frequency 50 Hz | 0.006269 W/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.01871 W/kg @Magnetic Field 0.200 T, Frequency 60 Hz | 0.008487 W/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0305 W/kg @Magnetic Field 0.300 T, Frequency 50 Hz | 0.0138 W/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0413 W/kg @Magnetic Field 0.300 T, Frequency 60 Hz | 0.0187 W/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0533 W/kg @Magnetic Field 0.400 T, Frequency 50 Hz | 0.0242 W/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0720 W/kg @Magnetic Field 0.400 T, Frequency 60 Hz | 0.0327 W/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0818 W/kg @Magnetic Field 0.500 T, Frequency 50 Hz | 0.0371 W/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.1103 W/kg @Magnetic Field 0.500 T, Frequency 60 Hz | 0.05003 W/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.1159 W/kg @Magnetic Field 0.600 T, Frequency 50 Hz | 0.05257 W/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.1556 W/kg @Magnetic Field 0.700 T, Frequency 50 Hz | 0.07058 W/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.1559 W/kg @Magnetic Field 0.600 T, Frequency 60 Hz | 0.07072 W/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.201 W/kg @Magnetic Field 0.800 T, Frequency 50 Hz | 0.0912 W/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.209 W/kg @Magnetic Field 0.700 T, Frequency 60 Hz | 0.0948 W/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.252 W/kg @Magnetic Field 0.900 T, Frequency 50 Hz | 0.114 W/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.269 W/kg @Magnetic Field 0.800 T, Frequency 60 Hz | 0.122 W/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.310 W/kg @Magnetic Field 1.00 T, Frequency 50 Hz | 0.141 W/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.337 W/kg @Magnetic Field 0.900 T, Frequency 60 Hz | 0.153 W/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.374 W/kg @Magnetic Field 1.10 T, Frequency 50 Hz | 0.170 W/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.413 W/kg @Magnetic Field 1.00 T, Frequency 60 Hz | 0.187 W/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.444 W/kg @Magnetic Field 1.20 T, Frequency 50 Hz | 0.201 W/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.498 W/kg @Magnetic Field 1.10 T, Frequency 60 Hz | 0.226 W/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.522 W/kg @Magnetic Field 1.30 T, Frequency 50 Hz | 0.237 W/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.592 W/kg @Magnetic Field 1.20 T, Frequency 60 Hz | 0.269 W/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.607 W/kg @Magnetic Field 1.40 T, Frequency 50 Hz | 0.275 W/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.696 W/kg @Magnetic Field 1.30 T, Frequency 60 Hz | 0.316 W/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.700 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz | 0.318 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.702 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz | 0.318 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.809 W/kg @Magnetic Field 1.40 T, Frequency 60 Hz | 0.367 W/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.811 W/kg @Magnetic Field 1.60 T, Frequency 50 Hz | 0.368 W/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.930 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz | 0.422 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.936 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz | 0.425 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.946 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | 0.429 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.950 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | 0.431 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 1.00 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | 0.454 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 1.079 W/kg @Magnetic Field 1.60 T, Frequency 60 Hz | 0.4894 W/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 1.145 W/kg @Magnetic Field 1.80 T, Frequency 50 Hz | 0.5194 W/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 1.16 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | 0.526 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.252 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | 0.5679 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.33 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | 0.603 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.506 W/kg @Magnetic Field 1.80 T, Frequency 60 Hz | 0.6831 W/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 1.551 W/kg @Magnetic Field 1.90 T, Frequency 50 Hz | 0.7035 W/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 2.02 W/kg @Magnetic Field 1.90 T, Frequency 60 Hz | 0.916 W/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
|
Descriptive Properties |
---|
Approximate Equivalent International Grade | M100-30P5 |
Magnetostriction 10^8 | -31 |
| -32 |
| -34 |
| -34 |
Maximum Induction at 800 A/m (T) | 1.88 |
Minimum Lamination Factor (%) | 95.5 |
Typical Induction at 800 A/m (T) | 1.917 |
Typical Lamination Factor (%) | 97.3 |