MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AK Steel TRAN-COR® H-2 CARLITE® DR® Grain Oriented Electrical Steel
Categories: Metal; Electronic/Magnetic Alloy; Ferrous Metal

Material Notes: TRAN-COR H CARLITE® high permeability electrical steels offer an outstanding degree of grain orientation, This combination of higher permeability with low residual stress offers the potential for lower core losses and less noisy transformer core structures, particularly at higher operating inductions, when compared to conventional grain oriented electrical steels. The core loss characteristics are further enhanced in the TRAN-COR H CARLITE DR® (Domain Refined) products where laser scribing is employed. In this process, a precisely focused laser beam is rapidly scanned across the steel surface. The micro-strain imparted into the material forces the pre-existing magnetic domains to subdivide. The finer domain structure reduces the distance that the domain walls must move during AC magnetization, thereby reducing eddy current losses. The result is far lower core loss than possible with conventional grain oriented electrical steels of comparable thickness. TRAN-COR H CARLITE products are suitable for all types of transformers while TRAN-COR H DR products are suitable for those types of transformers where a stress relief annealing treatment of the magnetic core is not used. Stress relief annealing will result in the eradication of the effect provided by the laser treatment and will result in a significant increase in core loss.

Information provided by AK Steel.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.65 g/cc
Thickness 270 - 310 microns
 300 micronsNominal
 
Mechanical PropertiesOriginal ValueComments
Knoop Microhardness 173
Hardness, Rockwell B 83
Tensile Strength, Ultimate 359 MPaIn rolling direction
Tensile Strength, Yield 345 MPaIn rolling direction
Elongation at Break 11 %In 2", rolling direction
Modulus of Elasticity 113.8 GPaIn rolling direction
 138 GPaAt 20° to rolling direction
 203 GPaAt 90° to rolling direction
 241 GPaAt 45° to rolling direction
 276 GPaAt 55° to rolling direction
 
Electrical PropertiesOriginal ValueComments
Exciting Power (RMS) 0.00270 RMS VA/lb
@Magnetic Field 0.100 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.00340 RMS VA/lb
@Magnetic Field 0.100 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.00950 RMS VA/lb
@Magnetic Field 0.200 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.0122 RMS VA/lb
@Magnetic Field 0.200 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.0199 RMS VA/lb
@Magnetic Field 0.300 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.0257 RMS VA/lb
@Magnetic Field 0.300 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.0335 RMS VA/lb
@Magnetic Field 0.400 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.0433 RMS VA/lb
@Magnetic Field 0.400 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.0496 RMS VA/lb
@Magnetic Field 0.500 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.0644 RMS VA/lb
@Magnetic Field 0.500 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.0684 RMS VA/lb
@Magnetic Field 0.600 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.0888 RMS VA/lb
@Magnetic Field 0.600 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.0897 RMS VA/lb
@Magnetic Field 0.700 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.1141 RMS VA/lb
@Magnetic Field 0.800 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.1168 RMS VA/lb
@Magnetic Field 0.700 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.1418 RMS VA/lb
@Magnetic Field 0.900 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.1482 RMS VA/lb
@Magnetic Field 0.800 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.1741 RMS VA/lb
@Magnetic Field 1.00 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.1841 RMS VA/lb
@Magnetic Field 0.900 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.2118 RMS VA/lb
@Magnetic Field 1.10 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.2264 RMS VA/lb
@Magnetic Field 1.00 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.2559 RMS VA/lb
@Magnetic Field 1.20 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.275 RMS VA/lb
@Magnetic Field 1.10 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.3086 RMS VA/lb
@Magnetic Field 1.30 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.3318 RMS VA/lb
@Magnetic Field 1.20 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.3718 RMS VA/lb
@Magnetic Field 1.40 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.3986 RMS VA/lb
@Magnetic Field 1.30 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.4514 RMS VA/lb
@Magnetic Field 1.50 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.4786 RMS VA/lb
@Magnetic Field 1.40 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.5609 RMS VA/lb
@Magnetic Field 1.60 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.5777 RMS VA/lb
@Magnetic Field 1.50 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.7118 RMS VA/lb
@Magnetic Field 1.60 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.7432 RMS VA/lb
@Magnetic Field 1.70 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.9318 RMS VA/lb
@Magnetic Field 1.70 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 1.2273 RMS VA/lb
@Magnetic Field 1.80 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 1.5045 RMS VA/lb
@Magnetic Field 1.80 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 4.4909 RMS VA/lb
@Magnetic Field 1.90 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 5.5682 RMS VA/lb
@Magnetic Field 1.90 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
Electrical Resistivity 0.0000500 ohm-cm
 
Magnetic PropertiesOriginal ValueComments
Core Loss 0.00361 W/kg
@Magnetic Field 0.100 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.00487 W/kg
@Magnetic Field 0.100 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.01382 W/kg
@Magnetic Field 0.200 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.01871 W/kg
@Magnetic Field 0.200 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.0305 W/kg
@Magnetic Field 0.300 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.0413 W/kg
@Magnetic Field 0.300 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.0533 W/kg
@Magnetic Field 0.400 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.0720 W/kg
@Magnetic Field 0.400 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.0818 W/kg
@Magnetic Field 0.500 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.1103 W/kg
@Magnetic Field 0.500 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.1159 W/kg
@Magnetic Field 0.600 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.1556 W/kg
@Magnetic Field 0.700 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.1559 W/kg
@Magnetic Field 0.600 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.201 W/kg
@Magnetic Field 0.800 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.209 W/kg
@Magnetic Field 0.700 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.252 W/kg
@Magnetic Field 0.900 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.269 W/kg
@Magnetic Field 0.800 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.310 W/kg
@Magnetic Field 1.00 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.337 W/kg
@Magnetic Field 0.900 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.374 W/kg
@Magnetic Field 1.10 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.413 W/kg
@Magnetic Field 1.00 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.444 W/kg
@Magnetic Field 1.20 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.498 W/kg
@Magnetic Field 1.10 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.522 W/kg
@Magnetic Field 1.30 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.592 W/kg
@Magnetic Field 1.20 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.607 W/kg
@Magnetic Field 1.40 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.696 W/kg
@Magnetic Field 1.30 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.700 W/kg
@Magnetic Field 1.50 T,
Frequency 50 Hz
Typical
 0.702 W/kg
@Magnetic Field 1.50 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.809 W/kg
@Magnetic Field 1.40 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.811 W/kg
@Magnetic Field 1.60 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.930 W/kg
@Magnetic Field 1.50 T,
Frequency 60 Hz
Typical
 0.936 W/kg
@Magnetic Field 1.50 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 0.946 W/kg
@Magnetic Field 1.70 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 0.950 W/kg
@Magnetic Field 1.70 T,
Frequency 50 Hz
Typical
 1.00 W/kg
@Magnetic Field 1.70 T,
Frequency 50 Hz
Maximum
 1.079 W/kg
@Magnetic Field 1.60 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 1.145 W/kg
@Magnetic Field 1.80 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 1.16 W/kg
@Magnetic Field 1.70 T,
Frequency 60 Hz
Typical
 1.252 W/kg
@Magnetic Field 1.70 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 1.33 W/kg
@Magnetic Field 1.70 T,
Frequency 60 Hz
Maximum
 1.506 W/kg
@Magnetic Field 1.80 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 1.551 W/kg
@Magnetic Field 1.90 T,
Frequency 50 Hz
ASTM A804, 0.30 mm
 2.02 W/kg
@Magnetic Field 1.90 T,
Frequency 60 Hz
ASTM A804, 0.30 mm
 
Descriptive Properties
Approximate Equivalent International GradeM100-30P5
Magnetostriction 10^8-31ASTM A876, 1.4T, 60Hz, 0.30 mm
 -32ASTM A876, 1.5T, 60Hz, 0.30 mm
 -34ASTM A876, 1.6T, 60Hz, 0.30 mm
 -34ASTM A876, 1.7T, 60Hz, 0.30 mm
Maximum Induction at 800 A/m (T)1.88
Minimum Lamination Factor (%)95.5
Typical Induction at 800 A/m (T)1.917
Typical Lamination Factor (%)97.3

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AK Steel DI-MAX® HF-10 Nonoriented Electrical Steel (Extended Electrical/Magnetic Data)
AK Steel CARLITE® M-3 Grain Oriented Electrical Steel
AK Steel DI-MAX® M-15 Nonoriented Electrical Steel
AK Steel DI-MAX® M-36 Nonoriented Electrical Steel
AK Steel DI-MAX® M-45 Nonoriented Electrical Steel

NAKS168 / 140764

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.