MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  
Rulon Bearings
Assab Steels 705M Machinery Steel
Categories: Metal; Ferrous Metal; Alloy Steel

Material Notes: ASSAB 705M is an alloyed machinery steel with good hardenability also in heavier sizes. As standard ASSAB 705M is supplied tough hardened with no further heat treatment required. It can be oil hardened to higher mechanical properties if required.

Applications: ASSAB 705M is suitable for induction hardening and can also be nitrided or tuffrided to a surface hardness of 600-650 Vickers.

ASSAB 705M is not suitable for welding but can with certain precautions be repair welded.

AISI /SAE 4340, DIN 34CrNiMo6, W.nr. 1.6582, BS 817M40 (EN 24), AFNOR 35NCD6, JIS SNCM8, SS 2541

Vendors:
Available Properties
  • Hardness, Brinell, 700°C tempering temperature. Quenching in oil ø 120. Test piece hardened by oil quenching from 850°C.
  • Hardness, Brinell, Hardness supplied approx.
  • Hardness, Brinell, 500°C tempering temperature. Quenching in oil ø 120. Test piece hardened by oil quenching from 850°C.
  • Hardness, Rockwell C, tempering temperature 500°C. Hardened by oil quenching.
  • Hardness, Rockwell C, 30 mm from the quenched end.
  • Hardness, Rockwell C, tempering temperature 200°C. Hardened by oil quenching.
  • Hardness, Rockwell C, 10 mm from the quenched end.
  • Tensile Strength at Break, Rm. 700°C tempering temperature. Quenching in oil ø 120. Test piece hardened by oil quenching from 850°C.
  • Tensile Strength at Break, Rm. 500°C tempering temperature. Quenching in oil ø 120. Test piece hardened by oil quenching from 850°C.
  • Tensile Strength, Ultimate, Rm
  • Tensile Strength, Yield, Re. 700°C tempering temperature. Quenching in oil ø 120. Test piece hardened by oil quenching from 850°C.
  • Tensile Strength, Yield, min. Re.
  • Tensile Strength, Yield, Re. 500°C tempering temperature. Quenching in oil ø 120. Test piece hardened by oil quenching from 850°C.
  • Elongation at Break
  • Elongation at Break, 5XD. 500°C tempering temperature. Quenching in oil ø 120. Test piece hardened by oil quenching from 850°C.
  • Elongation at Break, 5XD. 700°C tempering temperature. Quenching in oil ø 120. Test piece hardened by oil quenching from 850°C.
  • Reduction of Area, 500°C tempering temperature. Quenching in oil ø 120. Test piece hardened by oil quenching from 850°C.
  • Reduction of Area
  • Reduction of Area, 700°C tempering temperature. Quenching in oil ø 120. Test piece hardened by oil quenching from 850°C.
  • Impact Test
  • Carbon, C
  • Chromium, Cr
  • Iron, Fe
  • Manganese, Mn
  • Molybdenum, Mo
  • Nickel, Ni
  • Silicon, Si
  
Property Data

This page displays only the text
of a material data sheet.

To see MatWeb's complete data
sheet for this material (including
material property data, metal
compositions, material suppliers,
etc
), please click the button below.

Manufacturer Notes:
none

Category Notes
none

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

 

New MatWeb Services
Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.