MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
3D Systems LaserForm® 17-4PH (B) Stainless Steel Materials
Categories: Metal; 3D Printing/Additive Manufacturing Metal; Ferrous Metal; Tool Steel

Material Notes: Applications: Industrial grade prototypes, production parts or spare parts for:
  • Aerospace
  • Chemical and petrochemical industry
  • Energy sector
  • Surgical instruments
  • High-wear components
  • General metalworking
Features:
  • Outstanding combination of high strength and good corrosion resistance
  • Excellent mechanical properties at elevated temperatures — up to 300 °C
  • High hardness
  • Good thermal properties

Information provided by 3D Systems

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers 280 - 320As-Built
 380 - 420After Post Heat Treatment
Tensile Strength, Ultimate 1050 - 1150 MPaAs-Built; ASTM E8
 1250 - 1350 MPaAfter Post Heat Treatment; ASTM E8
Tensile Strength, Yield 590 - 650 MPaAs-Built; ASTM E8
 1050 - 1150 MPaAfter Post Heat Treatment; ASTM E8
Elongation at Break 8.0 - 12 %After Post Heat Treatment; ASTM E8
 14 - 18 %As-Built; ASTM E8
 
Component Elements PropertiesOriginal ValueComments
Chromium, Cr 15 - 17.5 %
Copper, Cu 3.0 - 5.0 %
Iron, Fe 70.05 - 78.85 %Balance
Manganese, Mn <= 1.0 %
Nickel, Ni 3.0 - 5.0 %
Niobium, Nb (Columbium, Cb) 0.15 - 0.45 %
Silicon, Si <= 1.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
ATI Allegheny Ludlum AL 17-4 High Strength Stainless Steel, UNS S17400
Latitude Manufacturing PowderFlo® 17-4PH Stainless Steel Metal Injection Molding Compound
Cast Stainless Steel 17- 4, UNS J92150 (Compostion Spec)
Carpenter Custom 630 (17-Cr-4Ni) Precipitation Hardening Stainless Steel, Condition H 1025 (Heated 552°C)
Proto Labs 17-4PH Stainless Steel - DMLS

PAPPR3000 / 238968

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.