MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Latitude Manufacturing PowderFlo® 17-4PH Stainless Steel Metal Injection Molding Compound  (discontinued **)
Categories: Metal; Ferrous Metal; Stainless Steel; Precipitation Hardening Stainless

Material Notes: Aqueous Agar Binder, Improved Gel Strength. Sintered properties are dependent on sintering conditions and specific parts. Sintered density > 98.5% is typical.

Metal injection molding (MIM) allows metal parts to be produced using standard injection molding machinery. This manufacturing process allows intricate metal parts to be produced that either can not be produced or are cost prohibitive to produce using other metal fabrication processes.

PowderFlo® MIM Compounds feature a patented aqueous agar-based binder system that is quickly and easily debound through simple air drying, offering an environmentally friendly production process. PowderFlo® MIM Compounds unique binder system also decreases limitations on part size and wall thickness that constrain the use of other MIM materials.

PowderFlo® is a registered trademark of Latitude Manufacturing Technologies. Information provided by Latitude Manufacturing Technologies.

Key Words: PM, Powder Metallurgy, Metal Powder MIM, 17-4 PH Stainless Steel
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density 4.60 g/cc0.166 lb/in³Feedstock; ASTM D792
Viscosity 100000 - 300000 cP100000 - 300000 cPFeedstock Capillary Viscosity at 1000 sec-1; ASTM D3835
Linear Mold Shrinkage 0.16 - 0.18 cm/cm0.16 - 0.18 in/inSintered Shrinkage for 0.40 in (10 mm) Section; ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C 3636Sintered and heat tempered at 1025°C; ASTM E18
 3838Sintered, HIP, and heat tempered at 1025°C; ASTM E18
Tensile Strength, Ultimate 1050 MPa152000 psiSintered and heat tempered at 1025°C; ASTM A370
 1140 MPa165000 psiSintered, HIP, and heat tempered at 1025°C; ASTM A370
Tensile Strength, Yield 979 MPa142000 psi0.2% Offset; Sintered and heat tempered at 1025°C; ASTM A370
 1100 MPa160000 psiSintered, HIP, and heat tempered at 1025°C; ASTM A370
Elongation at Break 10 %10 %Sintered and heat tempered at 1025°C; ASTM A370
 13 %13 %Sintered, HIP, and heat tempered at 1025°C; ASTM A370
Reduction of Area 23 %23 %Sintered and heat tempered at 1025°C; ASTM A370
 36 %36 %Sintered, HIP, and heat tempered at 1025°C; ASTM A370
 
Processing PropertiesMetricEnglishComments
Feed Temperature 71.1 - 93.3 °C160 - 200 °FInjection Cylinder
Mold Temperature 10.0 - 15.6 °C50.0 - 60.0 °F
Moisture Content 7.8 - 8.2 %7.8 - 8.2 %Feedstock
Injection Pressure 6.89 - 68.9 MPa1000 - 10000 psi
Sintering Temperature 1330 °C2430 °FHydrogen
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.070 %<= 0.070 %
Chromium, Cr 15 - 17.5 %15 - 17.5 %
Copper, Cu 3.0 - 3.5 %3.0 - 3.5 %
Iron, Fe 70.9 - 78.9 %70.9 - 78.9 %as balance
Manganese, Mn <= 1.0 %<= 1.0 %
Nickel, Ni 3.0 - 5.0 %3.0 - 5.0 %
Niobium, Nb (Columbium, Cb) 0.15 - 0.45 %0.15 - 0.45 %
Phosphorus, P <= 0.040 %<= 0.040 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.030 %<= 0.030 %

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Cast Stainless Steel 17- 4, UNS J92150 (Compostion Spec)
Carpenter Custom 630 (17-Cr-4Ni) Precipitation Hardening Stainless Steel, Annealed
Kinetics MIM 17-4PH Stainless Steel (As Sintered)
ATI Allvac® Vasco® 17-4 Precipitation Hardening Steel, Heat Treatment: 1038°C (1900°F) + Age
Kinetics MIM 17-4PH Stainless Steel (H1100 Condition)

N9RTP000 / 14578

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.