MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

USP Class VI Adhesives
USP Class VI Approved Adhesives for Medical Device Applications
Master Bond’s biocompatible adhesives are designed to meet the needs of medical device manufacturers. Compounds withstand various types of sterilization methods.

Epoxy Technology EPO-TEK® 354 High Temperature Epoxy
Categories: Polymer; Thermoset; Epoxy; Epoxy, High Temperature

Material Notes: Product Description: EPO-TEK® 354 is a two component, high Tg epoxy designed for semiconductor packaging in medical, fiber optic and optoelectronic assemblies. It is an electrically and thermally insulating epoxy.

Advantages & Application Notes:

  • Extended pot-life of many days which allows low waste between manufacturing shifts.
  • Built-in color change upon cure. Users can determine cure by visual means due to a red-amber color change from slight yellow.
  • Suggested Applications:
    • Semiconductor: capillary underfill below flip chip mounted die or SMDs.
    • Opto-electronic: %Transmission in the IR from 800 – 2000 nm range, adhesion to Si, glass, ceramic and metals.
    • Fiber Optic: sealing fiber into ferrules, optical connectors, adhesion to quartz, Au, kovar, stainless steel, packaging of Fiber Optic components.
    • Medical: resisting autoclave steam sterilization cycles in fiber optic bundles, adhesion to most plastics.
  • Designed to be a longer pot-life alternative to EPO-TEK® 353ND, it may be used in similar applications and devices.
  • Capable of being syringe dispensed in mass production. It’s medium viscosity lends itself to adhesive, sealing, potting and encapsulation.
  • Complies with USP Class VI biocompatibility standards.

Information Provided by Epoxy Technology

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.15 g/cc1.15 g/ccPart B
 1.20 g/cc1.20 g/ccPart A
Viscosity 4000 - 6000 cP
@Temperature 23.0 °C
4000 - 6000 cP
@Temperature 73.4 °F
50 rpm
 
Chemical PropertiesMetricEnglishComments
Ionic Impurities - Na (Sodium) 17 ppm17 ppm
Ionic Impurities - K (Potassium) 9.0 ppm9.0 ppm
Ionic Impurities - Cl (Chloride) 81 ppm81 ppm
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 8282
Tensile Modulus 2.46 GPa356 ksiStorage
Shear Strength 11.50 MPa1668 psiLap
 >= 23.4 MPa>= 3400 psiDie
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 2.00e+13 ohm-cm>= 2.00e+13 ohm-cm
Dielectric Constant 3.48
@Frequency 1000 Hz
3.48
@Frequency 1000 Hz
Dissipation Factor 0.0040
@Frequency 1000 Hz
0.0040
@Frequency 1000 Hz
 
Thermal PropertiesMetricEnglishComments
CTE, linear 96.0 µm/m-°C53.3 µin/in-°FBelow Tg
 175 µm/m-°C97.2 µin/in-°FAbove Tg
Maximum Service Temperature, Air 250 °C482 °FContinuous
 350 °C662 °FIntermittent
Minimum Service Temperature, Air -55.0 °C-67.0 °FContinuous
 -55.0 °C-67.0 °FIntermittent
Glass Transition Temp, Tg >= 95.0 °C>= 203 °FDynamic Cure 20—200°C /ISO 25 Min; Ramp 10—200°C @ 20°C/Min
Decomposition Temperature 487 °C909 °FDegradation Temperature
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.5734
@Wavelength 589 nm
1.5734
@Wavelength 589 nm
uncured
Transmission, Visible  >= 96 %
@Wavelength 600 nm
>= 96 %
@Wavelength 600 nm
Spectral
 >= 99 %
@Wavelength 800 nm
>= 99 %
@Wavelength 800 nm
Spectral
 
Processing PropertiesMetricEnglishComments
Cure Time  10.0 min
@Temperature 150 °C
0.167 hour
@Temperature 302 °F
Minimum Bond Line
 30.0 min
@Temperature 120 °C
0.500 hour
@Temperature 248 °F
Minimum Bond Line
Pot Life 180 min180 min
Shelf Life 12.0 Month
@Temperature 25.0 °C
12.0 Month
@Temperature 77.0 °F
 
Compliance PropertiesMetricEnglishComments
USP Class VI YesYes
 
Descriptive Properties
ColorClear/ColorlessPart A
 Dark AmberPart B
ConsistencyPourable liquid
Ionic Impurities NH4300 ppm
Mix Ratio by Weight10:1
Number of ComponentsTwo
Weight Loss0.5%200°C
 0.7%250°C
 0.85%300°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 413.0-F Die Casting Alloy
Hybrid Plastics POSS® EP 1050 Epoxy Adhesive
Chemical Concepts ChemSet™ CA5 Cyanoacrylate adhesive
Epoxy Technology EPO-TEK® 337H Graphite-Filled, High Temperature Epoxy
Epoxy Technology EPO-TEK® 353ND High Temperature Epoxy

PPOXYT129 / 141168

USP Class VI Adhesives
USP Class VI Approved Adhesives for Medical Device Applications
Master Bond’s biocompatible adhesives are designed to meet the needs of medical device manufacturers. Compounds withstand various types of sterilization methods.

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.