MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Solvay CYCOM® 950-1 Epoxy Prepreg with 38%-G7781
Categories: Polymer; Thermoset; Epoxy

Material Notes: CYCOM® 950-1 modified epoxy resin is a 121°C (250°F) cure system with the performance of a 177°C (350°F) curing epoxy. CYCOM 950-1 prepreg is curable under vacuum-bag-only pressure conditions. CYCOM 950-1 is a controlled flow, net resin content material that offers significant advantages over wet lay-up systems for structural repairs. Advantages include favorable stress-strain characteristics, product quality and consistency, speed of lay-up and vastly improved health and safety characteristics.

Features & Benefits:

  • Aerospace qualified
  • Low outgassing. Approved for space flight
  • Controlled flow material
  • Improved toughness compared with first- and second-generation structural epoxies
  • Dry service temperature of 150°C (300°F) when cured at 135°C (275°F)
  • Mechanical properties of a 177°C (350°F) curing material when cured at 135°C (275°F)
  • Mechanical properties to 104°C (220°F) hot/wet
  • Oven/vacuum bag cure capability as well as autoclave positive pressure cure
  • Efficient for structural repair
  • Conventional drying, lay-up, vacuum bagging and localized low-level heating is all that is required for most applications
  • Shop life of 8 weeks at ambient conditions
  • Suitable for laminate and sandwich panel usage
  • Co-curable with various aerospace qualified adhesive materials
Suggested Applications:
  • Helicopter fuselage and rotor components
  • Wing structures
  • Field repairs and permanent repairs
  • Space flight applications

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Outgassing - Total Mass Loss 0.24 %RML
 0.50 - 0.70 %TML
Collected Volatile Condensable Material 0.020 - 0.040 %
Storage Temperature <= -18.0 °C
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 34400 psi
@Temperature 121 °C
90° orientation
 40500 psi
@Temperature 93.0 °C
90° orientation
 46400 psi
@Temperature 121 °C
0° orientation
 49900 psi
@Temperature 93.0 °C
0° orientation
 54500 psi
@Temperature 24.0 °C
90° orientation
 67000 psi
@Temperature 24.0 °C
0° orientation
 69100 psi
@Temperature -55.0 °C
90° orientation
 79600 psi
@Temperature -55.0 °C
0° orientation
Tensile Modulus 12.5 GPa
@Temperature 121 °C
0° orientation
 14.6 GPa
@Temperature 121 °C
90° orientation
 16.6 GPa
@Temperature 93.0 °C
90° orientation
 20.5 GPa
@Temperature 93.0 °C
0° orientation
 20.6 GPa
@Temperature 24.0 °C
90° orientation
 22.6 GPa
@Temperature -55.0 °C
90° orientation
 23.0 GPa
@Temperature 24.0 °C
0° orientation
 25.8 GPa
@Temperature -55.0 °C
0° orientation
Flexural Strength 38800 psi
@Temperature 121 °C
0° orientation
 52900 psi
@Temperature 93.0 °C
0° orientation
 94000 psi
@Temperature 24.0 °C
0° orientation
 125500 psi
@Temperature -55.0 °C
0° orientation
Flexural Modulus 16.2 GPa
@Temperature 121 °C
0° orientation
 19.9 GPa
@Temperature 93.0 °C
0° orientation
 20.8 GPa
@Temperature -55.0 °C
0° orientation
 22.3 GPa
@Temperature 24.0 °C
0° orientation
Compressive Strength 232 MPa
@Temperature 121 °C
0° orientation
 233 MPa
@Temperature 121 °C
90° orientation
 274 MPa
@Temperature 93.0 °C
90° orientation
 352 MPa
@Temperature 93.0 °C
0° orientation
 428 MPa
@Temperature 24.0 °C
90° orientation
 500 MPa
@Temperature 24.0 °C
0° orientation
 510 MPa
@Temperature -55.0 °C
90° orientation
 630 MPa
@Temperature -55.0 °C
0° orientation
Shear Modulus 2.10 GPa
@Temperature 121 °C
In Plane
 5.00 GPa
@Temperature 93.0 °C
In Plane
 11.9 GPa
@Temperature 24.0 °C
In Plane
 16.1 GPa
@Temperature -55.0 °C
In Plane
Shear Strength 3000 psi
@Temperature 121 °C
Interlaminar
 4400 psi
@Temperature 93.0 °C
Interlaminar
 9700 psi
@Temperature -55.0 °C
Interlaminar
 9800 psi
@Temperature 24.0 °C
Interlaminar
 13900 psi
@Temperature 121 °C
In Plane
 17000 psi
@Temperature 93.0 °C
In Plane
 27700 psi
@Temperature 24.0 °C
In Plane
 38600 psi
@Temperature -55.0 °C
In Plane
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 220 °F
 
Processing PropertiesOriginal ValueComments
Gel Time 13.0 min
@Temperature 135 °C
Shelf Life 12.0 Month

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Solvay CYCOM® 919 Epoxy Prepreg System with Woven E Glass Fiber 7781
Park Aerospace Nelcote® E-722 Epoxy Prepreg, 7781 E-Glass Reinforced
Solvay CYCOM® 381 Epoxy E-glass Prepreg
Solvay CYCOM® 381 Epoxy Prepreg with E-glass Fabric and 300FAW Epoxy
Park Aerospace Nelcote® E-722 Epoxy Prepreg, 285 Kevlar® Reinforced

PCYTED154_3 / 192664

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.