MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Formosa Plastics Formolene® E924 Film HDPE
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Film Grade

Material Notes: High Molecular Weight High Density Polyethylene (HMW-HDPE) for Film Extrusion

Formolene® E924 is a bi-modal HMW-HDPE resin designed for high dart impact strength and good processing characteristics. Formolene® E924 is well balanced in overall physical properties and provides good stiffness for thin gauge film applications.

Formolene® E924 meets all requirements of the U.S. Food and Drug Administration as specified in 21 CFR 177.1520, covering safe use of polyolefin articles intended for direct food contact.

Applications: T-Shirt Bags, Industrial Liners, Trash Can Liners and Heavy Duty Bags

Information provided by Formosa Plastics Corporation, USA

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.949 g/cc0.0343 lb/in³ASTM D1505
Thickness 12.7 microns0.500 mil
Melt Flow 0.040 g/10 min
@Load 2.16 kg,
Temperature 190 °C
0.040 g/10 min
@Load 4.76 lb,
Temperature 374 °F
Condition E; ASTM D1238
High Load Melt Index 8.5 g/10 min
@Load 21.6 kg,
Temperature 190 °C
8.5 g/10 min
@Load 47.6 lb,
Temperature 374 °F
Condition F; ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Film Elongation at Break, MD 300 %300 %ASTM D882
Film Elongation at Break, TD 410 %410 %ASTM D882
Elmendorf Tear Strength MD 14 g14 gASTM D1922
Elmendorf Tear Strength TD 25 g25 gASTM D1922
Dart Drop Test 210 g0.463 lbASTM D1709
Film Tensile Strength at Break, MD 62.1 MPa9000 psiASTM D882
Film Tensile Strength at Break, TD 28.3 MPa4100 psiASTM D882
 
Thermal PropertiesMetricEnglishComments
Melting Point 131 °C268 °FDSC
 
Processing PropertiesMetricEnglishComments
Blow-up Ratio (BUR) 4.04.0
 
Compliance PropertiesMetricEnglishComments
FDA YesYesSee notes for details.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Petromont 7000 Medium Density Polyethylene Resin
Borealis FS1560 High Density Polyethylene
Baystar™ 2285 HDPE Bimodal Film Resin
Formosa Plastics Formolene® E924F Film HDPE
Formosa Plastics Formolene® L42022B Film (Butene Grade) LLDPE

PFPCPQ046 / 150278

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.