MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
CoorsTek Superstrate® TPS 99.6% Alumina Thin Film
Categories: Ceramic; Oxide; Aluminum Oxide

Material Notes: Applications: thin film substrates

Key Words: Al2O3
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 3.95 g/ccASTM-C373
Water Absorption 0.00 %ASTM-C373
Particle Size <= 1.0 µmGrain Size
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell 45 N 87ASTM-E18
Modulus of Elasticity 372 GPaASTM-C848
Flexural Strength 682 MPaASTM-F394
Poissons Ratio 0.20ASTM-C848
Shear Modulus 155 GPaCalculated
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+10 ohm-cm
@Temperature 700 °C
ASTM-D257
 >= 1.00e+12 ohm-cm
@Temperature 500 °C
ASTM-D257
 >= 1.00e+14 ohm-cm
@Temperature 300 °C
ASTM-D257
 >= 1.00e+15 ohm-cm
@Temperature 25.0 °C
ASTM-D257
 >= 1.00e+15 ohm-cm
@Temperature 100 °C
ASTM-D257
Dielectric Constant 9.9
@Frequency 1e+6 Hz
ASTM-D150
Dielectric Strength 500 V/mil
@Thickness 1.02 mm
ASTM-D149
 640 V/mil
@Thickness 0.635 mm
ASTM-D116
Dielectric Loss Index 0.00010
@Frequency 1e+6 Hz
 
Thermal PropertiesOriginal ValueComments
CTE, linear 6.30 µm/m-°C
@Temperature 25.0 - 300 °C
ASTM-C372
 7.20 µm/m-°C
@Temperature 25.0 - 600 °C
ASTM-C372
 7.90 µm/m-°C
@Temperature 25.0 - 800 °C
ASTM-C372
 8.20 µm/m-°C
@Temperature 25.0 - 1000 °C
ASTM-C372
Thermal Conductivity 27.0 W/m-K
@Temperature 100 °C
ASTM-C408
 
Component Elements PropertiesOriginal ValueComments
Al2O3 99.6 %
 
Descriptive Properties
ColorWhite
PermeabilityNIL
Surface Finish - (µin.)<1Polished; Profilometer, 0.004" Radius Stylus, 0.30" Cutoff, ANSI/ASME B46.1
 <10Lapped; Profilometer, 0.004" Radius Stylus, 0.30" Cutoff, ANSI/ASME B46.1

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DuPont Biomax® TPS 2700
DuPont Biomax® TPS 2501
DuPont Biomax® TPS 2100
Biomer P240 PHB Biodegradable Polymer
Biomer P209 PHB Biodegradable Polymer

CCOOR937 / 104641

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.