MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Astralloy 4145 H-Mod Alloy Steel Round Bars
Categories: Metal; Ferrous Metal; Alloy Steel

Material Notes:
  • Quenched and tempered for uniformity in strength, shock resistance, ductility and hardness.
  • Versatile machinery steel.
  • Furnished in a hot rolled state.
  • Minimum: 125 ksi yield.
  • Hardness: 287 – 332 BHN.
  • Mechanical properties at 1” below surface.

Information provided by Astralloy, a Nucor Company.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 287 - 332287 - 332
Tensile Strength 965 MPa140000 psi
Tensile Strength, Yield 862 MPa125000 psi
Elongation at Break 14 %
@Thickness 50.8 mm
14 %
@Thickness 2.00 in
Reduction of Area 45 %45 %
Charpy Impact 54.2 J40.0 ft-lb
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.49 %<= 0.49 %
Chromium, Cr <= 1.2 %<= 1.2 %
Iron, Fe >= 94.8 %>= 94.8 %As Balance
Manganese, Mn <= 1.3 %<= 1.3 %
Molybdenum, Mo <= 0.45 %<= 0.45 %
Nickel, Ni <= 1.0 %<= 1.0 %
Phosphorus, P <= 0.35 %<= 0.35 %
Silicon, Si <= 0.35 %<= 0.35 %
Sulfur, S <= 0.040 %<= 0.040 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI 4145 Steel
Astralloy 4330 V-Mod Alloy Steel Round Bars
AISI Type P20 Mold Steel (UNS T51620)
Ovako 42CrMo4-3 6107 (M) Steel, +QT
AISI 4145H Steel

NNUCOR916 / 233190

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.