MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Garlock GRAPH-LOCK® 3128 HOCHDRUCK® Graphite Sheet Gasketing, Steel Reinforced
Categories: Carbon; Graphite

Material Notes: High performance multi-layer graphite with 316SS inserts provides high compressive strength, blow-out resistance, excellent handling properties and improved tightness.
  • Pure exfoliated graphite flake material excels in extreme conditions, withstanding heat, pressure, and aggressive chemicals
  • Proven fire-safe
  • Seals easily under moderate bolt load, offers superior torque retention
  • Retains dimensional stability in high temperatures; seals tightly even during pressure fluctuations

Information provided by Garlock Rubber Technologies

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Permeability 0.40Gas Permeability, cc/min; DIN 3535 Part 4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 4500 psiASTM F152
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 1200 °FSteam
 850 °F
@Pressure 13.8 MPa
Minimum Service Temperature, Air -400 °F
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 99.85 %
 
Descriptive Properties
Compressibility, %30-40ASTM F36
Creep Relaxation, %10ASTM F38
Sealability ASTM F37B, ml/hr0.1Nitrogen
 0.2ASTM Fuel A

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Garlock THERMA-PUR™ 4122-KAMM High Temperature Gasketing Material
Garlock GRAPH-LOCK® 3124/3126 Graphite Sheet Gasketing, Steel Wire Insert
Garlock GYLON® 3530 PTFE Gasketing, Graphite Filler
Garlock THERMA-PUR™ 4122-CMG High Temperature Gasketing Material
Calcium Hydroxyapatite, Ca10(PO4)6(OH)2

PGARL841 / 157528

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.