MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
NOVA Chemicals Novapol® LC-0517-A LDPE Extrusion Resin  (discontinued **)
Categories: Polymer; Thermoplastic; Polyethylene (PE); Low Density (LDPE); Low Density Polyethylene (LDPE), Extrusion Grade

Material Notes: Excellent adhesion, High drawdown, Excellent sealability

Applications: Dry soup pouches, Powdered drink pouches, Pharmaceutical packaging, Potato chip bags, Flexible and snack food packaging

Additives: Base resin

Information provided by NOVA Chemicals.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.917 g/ccASTM D792
Water Vapor Transmission 18.0 g/m²/day
@Temperature 37.8 °C
90% RH; 30 lb Kraft paper samples with LDPE coating weight of 15 lb/ream; ASTM E96
Melt Flow 4.5 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238
Neck In 4.10 cmat 1000 ft/min; Neck-in reported is the total of both sides; NOVA Chemicals test method
Drawdown 5.10 m/sNOVA Chemical test method
Coating Weight >= 9.60 g/m²TAPPI test method; ASTM D539
 
Mechanical PropertiesOriginal ValueComments
Hot Tack Strength 225 g/25 mmTests done on samples with a coating weight of 12 lb/ream, prepared under the following extrusion coating conditions: Output Rate: 3 lb/hr/in, Melt Temp: 600°F, Die Width: 12 in, Substrate: 40 lb Kraft paper. Mfr reports 450 g per 50 mm (2 in).
Heat Seal Strength 1400 g/25 mmTests done on samples with a coating weight of 12 lb/ream, prepared under the following extrusion coating conditions: Output Rate: 3 lb/hr/in, Melt Temp: 600°F, Die Width: 12 in, Substrate: 40 lb Kraft paper; ASTM D517
 
Processing PropertiesOriginal ValueComments
Melt Temperature 315 - 325 °CUntreated substrate. Optimum adhesion is obtained at a draw span of about 10 cm.

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
NOVA Chemicals Novapol® LC-0522-A LDPE Extrusion Resin
NOVA Chemicals Novapol® LC-0717-A LDPE Extrusion Resin
Braskem BI 818 LDPE Injection Molding Polyethylene
Carmel Olefins Ipethene® 4203 Low Density Polyethylene
Chevron Phillips 4538B LDPE Injection Molding Resin

PNOVA128 / 55029

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.