System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
(Viewing data as-entered.
Click here
to return)
Envalior Durethan® BKV 215 H2.0 DUS008 901510 Nylon 6, Impact Modified
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 6 (PA6)
;
Nylon 6, Glass Filled, Impact Grade
Material Notes:
PA 6, 15% glass fibers, injection molding, impact modified, heat-aging stabilized
Former Lanxess product line is now with Envalior.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Specific Gravity
1.169
g/cc
ISO 1183
Linear Mold Shrinkage, Flow
0.00090
cm/cm
Post-shrinkage, 60x60x2; 120°C; 4 hour; ISO 294-4
0.0071
cm/cm
60x60x2; 280°C / MT 80°C; 600 bar; ISO 294-4
Linear Mold Shrinkage, Transverse
0.0015
cm/cm
Post-shrinkage, 60x60x2; 120°C; 4 hour; ISO 294-4
0.0075
cm/cm
60x60x2; 280°C / MT 80°C; 600 bar; ISO 294-4
Mechanical Properties
Original Value
Comments
Tensile Strength at Break
45.0
MPa
cond.; ISO 527-1, -2; 5 mm/min
80.0
MPa
d.a.m.; ISO 527-1, -2; 5 mm/min
Elongation at Break
5.0 %
d.a.m.; ISO 527-1, -2; 5 mm/min
15 %
cond.; ISO 527-1, -2; 5 mm/min
Tensile Modulus
2000
MPa
cond.; ISO 527-1, -2; 1 mm/min
4500
MPa
d.a.m.; ISO 527-1, -2; 1 mm/min
Flexural Strength
75.0
MPa
@Strain 8.0 %
cond., 2 mm/min; ISO 178-A
135
MPa
@Strain 5.5 %
d.a.m., 2 mm/min; ISO 178-A
Flexural Yield Strength
55.0
MPa
@Strain 3.5 %
cond., 2 mm/min; ISO 178-A
120
MPa
@Strain 3.5 %
d.a.m., 2 mm/min; ISO 178-A
Flexural Modulus
2100
MPa
cond., 2 mm/min; ISO 178-A
4100
MPa
d.a.m., 2 mm/min; ISO 178-A
Izod Impact, Notched (ISO)
10.0
kJ/m²
@Temperature -30.0 °C
d.a.m.; ISO 180-1A
10.0
kJ/m²
@Temperature -30.0 °C
cond.; ISO 180-1A
20.0
kJ/m²
@Temperature 23.0 °C
d.a.m.; ISO 180-1A
35.0
kJ/m²
@Temperature 23.0 °C
cond.; ISO 180-1A
Izod Impact, Unnotched (ISO)
60.0
kJ/m²
@Temperature 23.0 °C
d.a.m.; ISO 180-1U
60.0
kJ/m²
@Temperature -30.0 °C
cond.; ISO 180-1U
65.0
kJ/m²
@Temperature -30.0 °C
d.a.m.; ISO 180-1U
90.0
kJ/m²
@Temperature 23.0 °C
cond.; ISO 180-1U
Charpy Impact Unnotched
70.0
kJ/m²
@Temperature 23.0 °C
d.a.m.; ISO 179-1eU
80.0
kJ/m²
@Temperature -30.0 °C
d.a.m.; ISO 179-1eU
80.0
kJ/m²
@Temperature -30.0 °C
cond.; ISO 179-1eU
95.0
kJ/m²
@Temperature 23.0 °C
cond.; ISO 179-1eU
Charpy Impact, Notched
10.0
kJ/m²
@Temperature -30.0 °C
d.a.m.; ISO 179-1eA
10.0
kJ/m²
@Temperature -30.0 °C
cond.; ISO 179-1eA
20.0
kJ/m²
@Temperature 23.0 °C
d.a.m.; ISO 179-1eA
35.0
kJ/m²
@Temperature 23.0 °C
cond.; ISO 179-1eA
Thermal Properties
Original Value
Comments
Melting Point
219
°C
10°C/min; ISO 11357-1, -3
Deflection Temperature at 0.46 MPa (66 psi)
205
°C
ISO 75-1, -2
Deflection Temperature at 1.8 MPa (264 psi)
170
°C
ISO 75-1, -2
Processing Properties
Original Value
Comments
Melt Temperature
260
-
290
°C
280
°C
for test specimens; ISO 294
Mold Temperature
80.0
°C
for test specimens; ISO 294
80.0
-
100
°C
Drying Temperature
80.0
°C
Dry Time
2
-
6
hour
Moisture Content
0.030 - 0.12 %
residual; Karl Fischer Test
Descriptive Properties
ISO Short Name
ISO 1874-PA 6-HI, GHR, 14-040, GF15
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
Users viewing this material also viewed the following:
Envalior Durethan® BKY 115 H3.0 DUS008 Nylon 6, 15% Glass Fiber
Celanese Nilit Nilamid B3 H G3 15% Glass Fiber Reinforced PA6
Envalior Durethan® BKV 115 H3.0 000000 Nylon 6-Copolymer, Glass Fiber Reinforced
Ashley Polymers Ashlene® 525LD-13G Nylon 66, 13% Glass Reinforced
Ashley Polymers Ashlene® 527-25G Nylon 66, 25% Glass Reinforced
PLANX0627 / 133590
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.