Ashley Polymers Ashlene® 527-25G Nylon 66, 25% Glass Reinforced
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 66 (PA66)
;
Nylon 66, 30% Glass Fiber Filled
Material Notes:
A 25% glass reinforced impact modified Nylon 66.
Data provided by the manufacturer
Key Words:
Polyamide 66; Ashley Polymers, Inc.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.28
g/cc
0.0462
lb/in³
ASTM D792
Linear Mold Shrinkage
0.0050
cm/cm
0.0050
in/in
ASTM D955
Mechanical Properties
Metric
English
Comments
Tensile Strength, Ultimate
107
MPa
15500
psi
ATSM D638
Elongation at Break
4.0 %
4.0 %
ASTM D638
Flexural Modulus
5.20
GPa
754
ksi
ASTM D790
Izod Impact, Notched
1.60
J/cm
3.00
ft-lb/in
ASTM D256
Thermal Properties
Metric
English
Comments
Melting Point
252
°C
486
°F
ASTM D3418
Deflection Temperature at 0.46 MPa (66 psi)
218
°C
424
°F
ASTM D648
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Ashley Polymers Ashlene® 525LD-13G Nylon 66, 13% Glass Reinforced
Ashley Polymers Ashlene® 527LDMS Nylon 66
Ashley Polymers Ashlene® 527LD Nylon 66
Ashley Polymers Ashlene® 527LD-14G Nylon 66, 14% Glass Reinforced
Ashley Polymers Ashlene® 742L-13G Nylon 6/66, 13% Glass Reinforced
PNAA26 / 54373
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.