MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

(Viewing data as-entered. Click here to return)
Erbslöh Aluminium DISPAL S260 Aluminum Alloy, AlSi25Cu4Mg, Condition F
Categories: Metal; Nonferrous Metal; Aluminum Alloy

Material Notes: Excellent properties:
  • abrasive stability
  • high stiffness (E-modulus)
  • resistance even at high temperatures
  • good grindability

PEAK DISPAL materials allow the manufacturing of pistons for highest operational demands.

Information provided by PEAK Werkstoff GmbH, a part of Erbslöh Aluminium GmbH.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.527 - 2.793 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers >= 110
Tensile Strength at Break >= 87.0 MPa
@Temperature 300 °C
 >= 205 MPa
@Temperature 200 °C
 >= 265 MPa
@Temperature 20.0 °C
Tensile Strength, Yield >= 67.0 MPa
@Temperature 300 °C
 >= 144 MPa
@Temperature 200 °C
 >= 180 MPa
@Temperature 20.0 °C
Elongation at Break >= 1.0 %
@Temperature 20.0 °C
 >= 2.3 %
@Temperature 200 °C
 >= 15.3 %
@Temperature 300 °C
Modulus of Elasticity >= 48.0 GPa
@Temperature 300 °C
 >= 53.0 GPa
@Temperature 200 °C
 >= 85.0 GPa
@Temperature 20.0 °C
Poissons Ratio 0.277
@Temperature 20.0 °C
 0.279
@Temperature 100 °C
 0.279
@Temperature 150 °C
 0.281
@Temperature 200 °C
 0.282
@Temperature 300 °C
 0.283
@Temperature 250 °C
Fatigue Strength 189.1 MPaP50% rotary bending values for 5X107 cycles
 189.1 MPa
@# of Cycles 5.00e+7
P50% rotary bending value
Shear Modulus 31.0 GPa
@Temperature 300 °C
 32.0 GPa
@Temperature 250 °C
 33.0 GPa
@Temperature 200 °C
 34.0 GPa
@Temperature 100 °C
 34.0 GPa
@Temperature 100 °C
 35.0 GPa
@Temperature 20.0 °C
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000670 - 0.00000720 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 16.7 - 17.7 µm/m-°C
@Temperature 20.0 - 100 °C
 17.5 - 18.5 µm/m-°C
@Temperature 20.0 - 200 °C
 18.3 - 19.3 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.860 - 0.900 J/g-°C
Thermal Conductivity 124.1 W/m-K
@Temperature 400 °C
 131.5 W/m-K
@Temperature 200 °C
 131.9 W/m-K
@Temperature 300 °C
 132.7 W/m-K
@Temperature 100 °C
 135.5 W/m-K
@Temperature 30.0 °C
Melting Point 504 - 778 °C
Solidus 504.1 - 510.1 °C
Liquidus 772.1 - 778.1 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 70 %As Balance
Copper, Cu 4.0 %
Magnesium, Mg 1.0 %
Silicon, Si 25 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Erbslöh Aluminium DISPAL S220 Aluminum Alloy, AlSi35, Condition O
Erbslöh Aluminium DISPAL S260 Aluminum Alloy, AlSi25Cu4Mg, Condition T6
Erbslöh Aluminium DISPAL S260 Aluminum Alloy, AlSi25Cu4Mg, Condition T7
Erbslöh Aluminium DISPAL S693 Aluminum Alloy, AlCu5Ti, Condition T6
Erbslöh Aluminium DISPAL S225 Aluminum Alloy, AlSi35Fe2Ni, Condition F

NPEAK06 / 101611

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.