MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Hexcel® HexPly® F263 Epoxy Resin, 120 Glass Fabric
Categories: Polymer; Thermoset; Epoxy; Epoxy/Glass SMC

Material Notes: Hexcel designation: 120-38"-F263; Fiber: 450-1/2

Information provided by HexCel

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Filler Content 38.0 %Laminate Fiber Volume
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 263 MPa
@Temperature 177 °C
 368 MPa
@Temperature 24.0 °C
Tensile Modulus 20.3 GPa
@Temperature 177 °C
 23.9 GPa
@Temperature 24.0 °C
Compressive Yield Strength 345 MPa
@Temperature 177 °C
 474 MPa
@Temperature 24.0 °C
Compressive Modulus 21.4 GPa
@Temperature 177 °C
 23.5 GPa
@Temperature 24.0 °C
Shear Strength 21.0 MPa
@Temperature 24.0 °C
Interlaminar
 25.0 MPa
@Temperature 177 °C
Interlaminar
 
Descriptive Properties
Cured Thickness per Ply (cm)0.011Laminate
Dry Resin Content (%)42-48Prepreg
Flow (%)15-30

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Hexcel® HexPly® F185 Epoxy Resin, 120 Glass Fabric
Hexcel® F161 Epoxy Resin, 120 Glass Fabric
Hexcel® HexPly® F155 Epoxy Resin, 120 Glass Fabric
Hexcel® HexPly® F522 Epoxy Resin, 120 Glass Fabric
Hexcel® HexPly® M42 180°C (350°F) Curing Epoxy Matrix, 63%/120 E-Glass Fiber

PHEXC124 / 98594

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.