MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Celanese VECTRA V140 LCP, 40% Glass Reinforced
Categories: Polymer; Thermoplastic; Liquid Crystal Polymer (LCP); Liquid Crystal Polymer (LCP), 40% Glass Fiber Filled

Material Notes: LCP/PPS blend. Maintains most of the characteristics of A130 with improved weldline strength. 40% glass reinforced.
VECTRA should in principle be predried. Because of the necessary low maximum residual moisture content the use of dry air dryers is recommended. The dew point should be =< - 40° C. The time between drying and processing should be as short as possible.
For subsequent storage of the material in the dryer until processed the temperature does not need to be lowered for grades A, B, C, D and V (<= 24 h).

Information provided by Celanese Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.67 g/ccISO 1183
Linear Mold Shrinkage, Flow 0.0030 cm/cmISO 294-4
Linear Mold Shrinkage, Transverse 0.0060 cm/cmISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 96ISO 2039-2
Tensile Strength at Break 145 MPa5mm/min; ISO 527-2/1A
Tensile Stress at Strain 20.83 MPa
@Strain 0.13 %,
Temperature 23.0 °C
 37.89 MPa
@Strain 0.27 %,
Temperature 23.0 °C
 55.06 MPa
@Strain 0.41 %,
Temperature 23.0 °C
 70.68 MPa
@Strain 0.55 %,
Temperature 23.0 °C
 85.36 MPa
@Strain 0.69 %,
Temperature 23.0 °C
 99.77 MPa
@Strain 0.82 %,
Temperature 23.0 °C
 113.19 MPa
@Strain 0.96 %,
Temperature 23.0 °C
 124.9 MPa
@Strain 1.1 %,
Temperature 23.0 °C
 135.82 MPa
@Strain 1.24 %,
Temperature 23.0 °C
 145.38 MPa
@Strain 1.38 %,
Temperature 23.0 °C
Elongation at Break 1.0 %5mm/min; ISO 527-2/1A
Tensile Modulus 16000 MPa1mm/min; ISO 527-2/1A
Flexural Strength 230 MPaISO 178
Flexural Modulus 16000 MPaISO 178
Compressive Strength 134 MPa
@Strain 1 %
ISO 604
Compressive Modulus 16000 MPaISO 604
Izod Impact, Notched (ISO) 7.00 kJ/m²ISO 180/1A
Charpy Impact, Notched 11.0 kJ/m²ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+12 ohm-cmIEC 60093
Surface Resistance 1.00e+15 ohmIEC 60093
Dielectric Constant 3.7
@Frequency 1e+6 Hz
IEC 60250
 4.2
@Frequency 100 Hz
IEC 60250
Dielectric Strength 25.0 kV/mmIEC 60243-1
Dissipation Factor 0.0050
@Frequency 1e+6 Hz
IEC 60250
 0.020
@Frequency 100 Hz
IEC 60250
Arc Resistance 165 sec
Comparative Tracking Index 175 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 11.0 µm/m-°CISO 11359-2
CTE, linear, Transverse to Flow 21.0 µm/m-°CISO 11359-2
Melting Point 280 °CISO 11357-1,-2,-3
Deflection Temperature at 1.8 MPa (264 psi) 270 °CISO 75-1, -2
Flammability, UL94 V-0
@Thickness 0.400 mm
 V-0
@Thickness 1.50 mm
 
Processing PropertiesOriginal ValueComments
Processing Temperature 20.0 - 30.0 °Chopper
 80.0 - 120 °Ccavity
Feed Temperature 60.0 - 80.0 °C
Zone 1 295 - 305 °C
Zone 2 300 - 310 °C
Zone 3 300 - 310 °C
Zone 4 300 - 310 °C
Die Temperature 300 - 310 °C
Melt Temperature 293 °CISO 294
 300 - 315 °C
Mold Temperature 100 °CISO 294
Injection Velocity 150 mm/secISO 294
Drying Temperature 150 °C
Dry Time 4 - 24.0 hour
Moisture Content 0.010 %Necessary low maximum
Injection Pressure 69.0 MPaISO 294
 7250 - 21750 psi
Hold Pressure 7250 - 21750 psi
Back Pressure <= 435 psi
Screw Speed 80 rpm
@Diameter 40.0 mm
 140 rpm
@Diameter 25.0 mm
 200 rpm
@Diameter 16.0 mm
Hot-Working Temperature 300 - 310 °C
 
Descriptive Properties
Injection moldingYes
Injection speedvery fast
RemarksWhen using short metering strokes an accumulator is recommended to get short injection times

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Schott BG60 Bandpass Filter
Celanese Vectra® V140 Liquid Crystal Polymer (LCP), 40% Glass Reinforced
Celanese VECTRA S135 LCP, 35% Glass Reinforced
Schott IRG 24 Infrared Chalcogenide Glass

PHCS495 / 123910

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.