MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Flint Hills P5M6K-080 Polypropylene Random Copolymer
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene Copolymer

Material Notes: Features: Clarified, Gamma Radiation Sterilizable. Product does not contain animal derived components. Phthalate-free.

Applications: Injection molding: Disposable Syringes. This product is not recommended for autoclave sterilization processes in the presence of aqueous solutions.

Information Provided by Flint Hills Resources

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.900 g/ccASTM D1505
Melt Flow 27 g/10 minASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 85ASTM D785
Tensile Strength, Yield 31.0 MPaASTM D638
Elongation at Yield 14 %ASTM D638
Flexural Modulus, 1% Secant 966 MPaASTM D790
Izod Impact, Notched 75.0 J/m
@Temperature 23.0 °C
ASTM D256
Gardner Impact 27.0 J
@Temperature 23.0 °C
ASTM D5420
Tangent Modulus 1000 MPaASTM D790
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 81.0 °CASTM D648
 
Optical PropertiesOriginal ValueComments
Haze 13 %
@Thickness 1.27 mm
ASTM D1003

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Ineos H28U-00 Polypropylene Homopolymer
Total PPH 3620WZ Polypropylene, Injection Molding Grade
Borealis Bormed™ HD810MO Polypropylene Copolymer for Medical Applications
Total PPH 3740WR Polypropylene, High Flow Nucleated Homopolymer Injection Molding
Flint Hills P5L2K-055 Polypropylene Random Copolymer

PFLINT028 / 104582

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.