MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Nickel Aluminum Bronze, UNS C63000, HR50 Temper
Categories: Metal; Nonferrous Metal; Copper Alloy; Bronze

Material Notes: Good to excellent corrosion resistance. Good hot formability. Fabricated by hot forming and forging.

Applications: nuts, bolts, valve seats, plunger tips, marine shafts, valve guides, aircraft parts, pump shafts, structural members.

Properties typical for 25mm diameter round rod.

Key Words: CDA 630, CA104, ISO CuAl10Ni5Fe4, Aluminum Bronze E, 82Cu-10Al-5Ni-3Fe
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 7.58 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 94
Tensile Strength, Ultimate 760 MPa
Tensile Strength, Yield 470 MPa
Elongation at Break 10 %in 50 mm, 10% reduction in area
Modulus of Elasticity 115 GPa
Compressive Strength 1035 MPa
Poissons Ratio 0.328
Fatigue Strength 255 MPa
@# of Cycles 1.00e+8
Reverse Bending; Temper Not Reported
Machinability 30 %UNS C36000 (free-cutting brass) = 100%
Forgeability 75 %
Shear Modulus 44.0 GPa
Charpy Impact 16.0 - 21.0 JV-notch
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000192 ohm-cm
@Temperature 20.0 °C
Magnetic Permeability 1.05
 
Thermal PropertiesOriginal ValueComments
CTE, linear 16.2 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.375 J/g-°C
Thermal Conductivity 37.7 W/m-K
@Temperature 20.0 °C
Melting Point 1035 - 1055 °C
Solidus 1035 °C
Liquidus 1055 °C
Annealing Point 1100 - 1300 °F
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 600 - 700 °C
Hot-Working Temperature 800 - 925 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 9.0 - 11 %
Copper, Cu 78 - 85 %
Iron, Fe 2.0 - 4.0 %
Manganese, Mn <= 1.5 %
Nickel, Ni 4.0 - 5.5 %Includes Co
Other, total <= 0.50 %
Silicon, Si <= 0.25 %
Tin, Sn <= 0.20 %
Zinc, Zn <= 0.30 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum Bronze, UNS C61300, Annealed
Nickel Aluminum Bronze, UNS C63000, Annealed Rod
Nickel Aluminum Bronze, UNS C63000, Cold Finished Rod
Aluminum Bronze D, UNS C61400, Annealed Rod
Ampco Metal AMPCO® 45 Nickel-Aluminum Bronze, Extruded and Drawn Rods, ≤ 25.4 mm.

MC63000b1 / 11611

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.