MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Ampco Metal CuAl10Ni5Fe4 Aluminum Bronze, Extruded Rod
Categories: Metal; Nonferrous Metal; Copper Alloy; Bronze

Material Notes: Aluminum bronze extruded rods

Applications: Construction material with good strength properties, sea water resistant. Endless screws with high tooth pressures and good lubrication.

Key Words: CDA C63000; DIN 17665 CuAl10Ni5Fe4 2.0966; AFNOR CuAl9Ni5Fe3M1
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.60 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 180HB 10
Tensile Strength, Ultimate 640 MPa
Tensile Strength, Yield 270 MPa
@Strain 0.2 %
Elongation at Break 15 %
Modulus of Elasticity 121 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000250 ohm-cm7% I.A.C.S.
 
Thermal PropertiesOriginal ValueComments
CTE, linear 16.2 µm/m-°C
@Temperature 20.0 °C
Specific Heat Capacity 0.450 J/g-°C
Thermal Conductivity 40.0 W/m-K
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 8.5 - 11 %
Copper, Cu 76.5 - 85.5 %As Balance
Iron, Fe 2.0 - 5.0 %
Manganese, Mn <= 1.5 %
Nickel, Ni 4.0 - 6.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Nickel Aluminum Bronze, UNS C63000, Annealed Rod
Nickel Aluminum Bronze, UNS C63000, Cold Finished Rod
Nickel Aluminum Bronze, UNS C63000, HR50 Temper
Chicago Extruded Metals BioBrass® UNS C63000 Aluminum Bronze
420 Stainless Steel, hardened and tempered bar

NAMPCO61 / 15015

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.