MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metal adhesives

(Viewing data as-entered. Click here to return)
3M Bumpon™ SJ6008 Resilient Rollstock
Categories: Polymer; Adhesive

Material Notes: 3M Bumpon Resilient Rollstock Products are opaque, colored polyurethane materials produced with aggressive pressure-sensitive adhesives.

Information provided by 3M

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.30 g/cc
Thickness 125 mil
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore M 72Polyurethane
Tensile Strength at Break 4.14 MPaDie A; ASTM D412
Elongation at Break 100 %Die A; ASTM D412
Coefficient of Friction, Dynamic >= 1.0Stainless Steel
 >= 1.0Glass
 0.90 - 1.4Formica laminate
 0.90 - 1.4Wood
Peel Strength 3.00 pli90°, Adhesion to Polypropylene
 11.0 pli90°, Adhesion to Polystyrene
 25.0 pli90°, Adhesion to ABS
 25.0 pli90°, Adhesion to Stainless Steel
 25.0 pli90°, Adhesion to Aluminum
Taber Abrasion, mg/1000 Cycles 1.7 - 1.9H18, 1 kg; ASTM C501
Compression Set 3.0 %ASTM D1056
 4.0 %25% deflection; ASTM D1056
 
Electrical PropertiesOriginal ValueComments
Dielectric Strength 200 kV/inASTM D1000
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 66.0 °C
 107 °CIntermittent Exposure
Minimum Service Temperature, Air -34.0 °C
Flammability, UL94 HB
 
Processing PropertiesOriginal ValueComments
Processing Temperature >= 5.00 °CApplication
 <= 52.0 °CApplication
 
Descriptive Properties
Adhesive TypeA-20 (acrylic)
AppearanceBlack Brown

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PMM35226 / 169973

Metal adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.