MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Schmolz + Bickenbach Thermodur® 2999 Hot Work Die Steel
Categories: Metal; Ferrous Metal; Tool Steel; Hot Work Steel

Material Notes: Description: Maximum high-temperature strength, good high-temperature wear resistance, excellent thermal shock resistance and thermal conductivity across the entire range of service temperatures

Applications: Die inserts and high-speed forging tools exposed to severe wear stresses, heavy metal die casting, hot-work tool steels for use at highest temperatures.

Hardening (Heat Treatment): 1070°C- 1100°C; Quenching: Oil or hot bath, 500-550°C; Hardness: 57 HRC Quenched

Information provided by Schmolz + Bickenbach

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C  46
@Treatment Temp. 650.0 °C
46
@Treatment Temp. 1202 °F
 53
@Treatment Temp. 600.0 °C
53
@Treatment Temp. 1112 °F
 54
@Treatment Temp. 200 °C
54
@Treatment Temp. 392 °F
 54
@Treatment Temp. 300 °C
54
@Treatment Temp. 572 °F
 55
@Treatment Temp. 100 °C
55
@Treatment Temp. 212 °F
 55
@Treatment Temp. 400 °C
55
@Treatment Temp. 752 °F
 56
@Treatment Temp. 500 °C
56
@Treatment Temp. 932 °F
 57
@Treatment Temp. 550.0 °C
57
@Treatment Temp. 1022 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.3 µm/m-°C
@Temperature 20.0 - 100 °C
6.28 µin/in-°F
@Temperature 68.0 - 212 °F
 11.9 µm/m-°C
@Temperature 20.0 - 200 °C
6.61 µin/in-°F
@Temperature 68.0 - 392 °F
 12.2 µm/m-°C
@Temperature 20.0 - 300 °C
6.78 µin/in-°F
@Temperature 68.0 - 572 °F
 12.6 µm/m-°C
@Temperature 20.0 - 400 °C
7.00 µin/in-°F
@Temperature 68.0 - 752 °F
 13.0 µm/m-°C
@Temperature 20.0 - 500 °C
7.22 µin/in-°F
@Temperature 68.0 - 932 °F
 13.3 µm/m-°C
@Temperature 20.0 - 600.0 °C
7.39 µin/in-°F
@Temperature 68.0 - 1112 °F
 13.5 µm/m-°C
@Temperature 20.0 - 700.0 °C
7.50 µin/in-°F
@Temperature 68.0 - 1292 °F
Thermal Conductivity  31.4 W/m-K
@Temperature 20.0 °C
218 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
Quenched and Tempered
 35.2 W/m-K
@Temperature 350 °C
244 BTU-in/hr-ft²-°F
@Temperature 662 °F
Quenched and Tempered
 36.2 W/m-K
@Temperature 700.0 °C
251 BTU-in/hr-ft²-°F
@Temperature 1292 °F
Quenched and Tempered
 37.8 W/m-K
@Temperature 20.0 °C
262 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
Annealed
 39.5 W/m-K
@Temperature 350 °C
274 BTU-in/hr-ft²-°F
@Temperature 662 °F
Annealed
 39.5 W/m-K
@Temperature 700.0 °C
274 BTU-in/hr-ft²-°F
@Temperature 1292 °F
Annealed
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 399 - 427 °C750 - 800 °FSoft; Cooling: Furnace; <230 HB
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.45 %0.45 %
Chromium, Cr 3.0 %3.0 %
Iron, Fe 89.95 %89.95 %
Manganese, Mn 0.30 %0.30 %
Molybdenum, Mo 5.0 %5.0 %
Silicon, Si 0.30 %0.30 %
Vanadium, V 1.0 %1.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Bohler-Uddeholm ORVAR® 2M / AISI H13 Hot Work Tool Steel
Schmolz + Bickenbach Formadur® PH X Superclean Plastic Mold Steel
Assab Steels HOTVAR Hot Work Steel
Bohler-Uddeholm UDDEHOLM ORVAR® SUPERIOR (Premium AISI H13) Hot Work Tool Steel
Carpenter Extendo-Die® Hot Work Die Steel, Tempered 560°C

NSCHMO018 / 125891

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.