MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Schmolz + Bickenbach Formadur® PH X Superclean Plastic Mold Steel
Categories: Metal; Ferrous Metal; Martensitic; Tool Steel; Mold Steel

Material Notes: Description: Formadur® PH X Superclean is a corrosion-resistant, martensitic precipitation hardened stainless steel

Characteristics: Excellent resistance to corrosion; Excellent polishability; Excellent dimensional stability; Good strength; and Good toughness

Applications: Formadur® PH X Superclean is recommended for tools/molds for the processing of corrosive plastics.

Information provided by Schmolz + Bickenbach

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.89 g/cc0.285 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C  34
@Treatment Temp. 593 °C,
Time 14400 sec
34
@Treatment Temp. 1100 °F,
Time 4.00 hour
 38
@Treatment Temp. 551.7 °C,
Time 14400 sec
38
@Treatment Temp. 1025 °F,
Time 4.00 hour
 41
@Treatment Temp. 496 °C,
Time 14400 sec
41
@Treatment Temp. 925 °F,
Time 4.00 hour
 42
@Treatment Temp. 399 °C,
Time 14400 sec
42
@Treatment Temp. 750 °F,
Time 4.00 hour
 43
@Treatment Temp. 454 °C,
Time 14400 sec
43
@Treatment Temp. 850 °F,
Time 4.00 hour
 44
@Treatment Temp. 482 °C,
Time 14400 sec
44
@Treatment Temp. 900 °F,
Time 4.00 hour
Tensile Strength 1120 MPa162000 psi38 HRC
 1190 MPa172000 psi40 HRC
 1240 MPa180000 psi42 HRC
Tensile Strength, Yield  1100 MPa
@Strain 0.2 %
160000 psi
@Strain 0.2 %
38 HRC
 1170 MPa
@Strain 0.2 %
170000 psi
@Strain 0.2 %
40 HRC
 1210 MPa
@Strain 0.2 %
175000 psi
@Strain 0.2 %
42 HRC
Elongation at Yield 12.2 %12.2 %40 HRC
 12.2 %12.2 %42 HRC
 12.8 %12.8 %38 HRC
Charpy Impact 33.9 J25.0 ft-lbNotched; at 38 HRC
 
Thermal PropertiesMetricEnglishComments
CTE, linear  10.6 µm/m-°C
@Temperature 21.1 - 93.3 °C
5.90 µin/in-°F
@Temperature 70.0 - 200 °F
 10.8 µm/m-°C
@Temperature 21.1 - 204 °C
6.00 µin/in-°F
@Temperature 70.0 - 400 °F
 16.6 µm/m-°C
@Temperature 21.1 - 399 °C
9.20 µin/in-°F
@Temperature 70.0 - 750 °F
Thermal Conductivity  16.6 W/m-K
@Temperature 21.1 °C
115 BTU-in/hr-ft²-°F
@Temperature 70.0 °F
 18.0 W/m-K
@Temperature 149 °C
125 BTU-in/hr-ft²-°F
@Temperature 300 °F
 22.3 W/m-K
@Temperature 504 °C
155 BTU-in/hr-ft²-°F
@Temperature 940 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.050 %0.050 %
Chromium, Cr 15 %15 %
Copper, Cu 3.5 %3.5 %
Iron, Fe 76.95 %76.95 %
Nickel, Ni 4.5 %4.5 %
 
Descriptive Properties
Corrosion Properties/Weight loss rate0.2% Hydrochloric Acid0.0017 g/hm2
 5% Acetic Acid0.018 g/hm2
 5% Nitric Acid0.0015 g/hm2
 5% Sulfuric Acid5 g/hm2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI Type 316F Stainless Steel, annealed bar
Schmolz + Bickenbach Formadur® 2083 Superclean Plastic Mold Steel
Schmolz + Bickenbach P-20 High Hard Plastic Mold Steel
Schmolz + Bickenbach CorroPlast® Plastic Mold Steel
AISI Type S13800 Stainless Steel (PH 13-8 Mo) longitudinal properties, condition RH950

NSCHMO009 / 125882

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.