MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
BASF Ultrason® P 3010 PPSU Unreinforced Polyphenylsulfone
Categories: Polymer; Thermoplastic; Polyphenylsulfone (PPSU)

Material Notes: Description: Medium viscosity injection-molding and extrusion grade with good toughness and chemical resistance (stress crack resistance), resistant against superheated steam. The property profile makes it possible to use them in high-quality technical components and heavy-duty mass products. Conventional processing methods for thermoplastics can be applied. Ultrason® can thus be used where, for example, polyamide, polycarbonate, polyoxymethylene, and polyalkylene terephthalate are no longer suitable, primarily due to thermal or hydrolytic instability. The property spectrum of Ultrason® products allows the substitution of duromers, metals, and ceramics.

Information provided by BASF

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Bulk Density 0.700 - 0.800 g/cc
Density 1.29 g/ccISO 1183
Water Absorption <= 1.2 %Equilibrium; ISO 62
 0.56 %
@Thickness 2.00 mm,
Time 180000 sec
Storage; ISO 62
 1.0 %
@Thickness 2.00 mm,
Time 360000 sec
Storage; ISO 62
 1.15 %
@Thickness 2.00 mm,
Time 1.08e+6 sec
Storage; ISO 62
 1.2 %
@Thickness 2.00 mm,
Time 1.80e+6 sec
Storage; ISO 62
Moisture Absorption at Equilibrium 0.60 %23°C; 50% RH; ISO 62
Water Vapor Transmission 100 - 150 g/m²/dayDIN EN 12086
Viscosity Measurement 71Viscosity number; ISO 1628
Linear Mold Shrinkage, Flow 0.0090 cm/cmISO 294
Linear Mold Shrinkage, Transverse 0.010 cm/cmISO 294
Melt Flow >= 45.15 g/10 min
@Load 10.0 kg,
Temperature 360 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 124 MPa
@Load 36.5 kg,
Time 30.0 sec
ISO 2039-1
Tensile Strength at Break 74.0 MPa5 mm/min; ISO 527-2
Tensile Stress 30.0 MPa
@Temperature 160 °C
 35.0 MPa
@Temperature 160 °C
 40.0 MPa
@Temperature 23.0 °C
 60.0 MPa
@Temperature 23.0 °C
 70.0 MPa
@Temperature 23.0 °C
Tensile Strength, Yield 74.0 MPa50 mm/min; ISO 527-2
 45.0 MPa
@Temperature 140 °C
 55.0 MPa
@Temperature 100 °C
 65.0 MPa
@Temperature 60.0 °C
 75.0 MPa
@Temperature 20.0 °C
Elongation at Break 7.8 %5mm/min; ISO 527-2
Elongation at Yield 7.8 %50 mm/min; ISO 527-2
 0.18 %
@Time 36000 sec,
Pressure 30.0 MPa
ISO 899
 0.20 %
@Time 3600 sec,
Pressure 6.00 MPa
180°C; ISO 899
 0.28 %
@Time 36000 sec,
Pressure 42.0 MPa
ISO 899
 0.40 %
@Time 3600 sec,
Pressure 8.00 MPa
180°C; ISO 899
 0.50 %
@Pressure 6.00 MPa,
Time 360000 sec
180°C; ISO 899
 0.50 %
@Time 3600 sec,
Pressure 10.0 MPa
ISO 899
 0.51 %
@Pressure 10.0 MPa,
Time 36000 sec
ISO 899
 0.52 %
@Pressure 10.0 MPa,
Time 360000 sec
ISO 899
 0.53 %
@Pressure 10.0 MPa,
Time 3.60e+6 sec
ISO 899
 0.90 %
@Time 3600 sec,
Pressure 12.0 MPa
180°C; ISO 899
 1.0 %
@Time 3600 sec,
Pressure 14.0 MPa
180°C; ISO 899
 1.0 %
@Pressure 6.00 MPa,
Time 3.60e+6 sec
180°C; ISO 899
 1.0 %
@Pressure 8.00 MPa,
Time 360000 sec
180°C; ISO 899
 1.1 %
@Time 3600 sec,
Pressure 16.0 MPa
180°C; ISO 899
 1.1 %
@Time 3600 sec,
Pressure 20.0 MPa
ISO 899
 1.2 %
@Time 36000 sec,
Pressure 20.0 MPa
ISO 899
 1.25 %
@Pressure 20.0 MPa,
Time 360000 sec
ISO 899
 1.28 %
@Pressure 20.0 MPa,
Time 3.60e+6 sec
ISO 899
 1.75 %
@Time 3600 sec,
Pressure 30.0 MPa
ISO 899
 1.9 %
@Pressure 8.00 MPa,
Time 3.60e+6 sec
180°C; ISO 899
 1.9 %
@Pressure 12.0 MPa,
Time 360000 sec
180°C; ISO 899
 1.95 %
@Pressure 30.0 MPa,
Time 360000 sec
ISO 899
 2.1 %
@Pressure 30.0 MPa,
Time 3.60e+6 sec
ISO 899
 2.1 %
@Pressure 14.0 MPa,
Time 360000 sec
180°C; ISO 899
 2.5 %
@Time 3600 sec,
Pressure 40.0 MPa
ISO 899
 2.6 %
@Time 36000 sec,
Pressure 40.0 MPa
ISO 899
 2.7 %
@Pressure 40.0 MPa,
Time 360000 sec
ISO 899
 2.75 %
@Time 3600 sec,
Pressure 42.0 MPa
ISO 899
 3.0 %
@Pressure 16.0 MPa,
Time 360000 sec
180°C; ISO 899
 3.0 %
@Pressure 40.0 MPa,
Time 3.60e+6 sec
ISO 899
 3.0 %
@Pressure 42.0 MPa,
Time 360000 sec
ISO 899
 3.2 %
@Pressure 42.0 MPa,
Time 3.60e+6 sec
ISO 899
 3.5 %
@Pressure 12.0 MPa,
Time 3.60e+6 sec
180°C; ISO 899
 4.5 %
@Pressure 14.0 MPa,
Time 3.60e+6 sec
180°C; ISO 899
 5.5 %
@Pressure 16.0 MPa,
Time 3.60e+6 sec
180°C; ISO 899
Creep Strength 30.0 MPa
@Time 3.60e+7 sec
in water at 95°C
 33.0 MPa
@Time 3.60e+6 sec
in water at 95°C
 35.0 MPa
@Time 360000 sec
in water at 95°C
 37.0 MPa
@Time 36000 sec
in water at 95°C
Modulus of Elasticity 1.60 GPa
@Temperature 140 °C
ISO 527
 1.90 GPa
@Temperature 100 °C
ISO 527
 2.10 GPa
@Temperature 60.0 °C
ISO 527
 2.25 GPa
@Temperature 20.0 °C
ISO 527
Tensile Modulus >= 2270 MPaISO 527-2
 >= 1600 MPa
@Temperature 140 °C
Elasticity
 >= 1900 MPa
@Temperature 100 °C
Elasticity
 >= 2100 MPa
@Temperature 60.0 °C
Elasticity
 >= 2250 MPa
@Temperature 20.0 °C
Elasticity
Shear Modulus 0.200 GPa
@Temperature 225 °C
ISO 6721
 0.700 GPa
@Temperature 200 °C
ISO 6721
 0.750 GPa
@Temperature 150 °C
ISO 6721
 0.775 GPa
@Temperature 100 °C
ISO 6721
 0.800 GPa
@Temperature 50.0 °C
ISO 6721
Adhesive Bond Strength >= 0.200 MPaon plastic
Izod Impact, Notched (ISO) 22.0 kJ/m²
@Temperature -60.0 °C
ISO 179/1eA
 24.0 kJ/m²
@Temperature -40.0 °C
ISO 179/1eA
 41.0 kJ/m²
@Temperature -25.0 °C
ISO 179/1eA
 60.0 kJ/m²
@Temperature -20.0 °C
ISO 179/1eA
 61.0 kJ/m²
@Temperature 0.000 °C
ISO 179/1eA
 65.0 kJ/m²
@Temperature 20.0 °C
ISO 179/1eA
 65.0 kJ/m²
@Temperature 40.0 °C
ISO 179/1eA
 70.0 kJ/m²
@Temperature 0.000 °C
ISO 179/1eA
 85.0 kJ/m²
@Temperature 50.0 °C
ISO 179/1eA
 87.0 kJ/m²
@Temperature 100 °C
ISO 179/1eA
Charpy Impact Unnotched NB
@Temperature -30.0 °C
ISO 179/1eU
 NB
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched 25.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
 65.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+13 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohmIEC 60093
Dielectric Constant 3.7
@Frequency 1e+6 Hz
ISO 60250
 3.8
@Frequency 100 Hz
ISO 60250
Dielectric Strength 44.0 kV/mmIEC 60243-13
Dissipation Factor 0.00170
@Frequency 100 Hz
IEC 60250
 0.0089
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 150 VTest Liquid A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear 55.0 µm/m-°C
@Temperature 25.0 °C
DIN 53752
 57.0 µm/m-°C
@Temperature 75.0 °C
DIN 53752
 60.0 µm/m-°C
@Temperature 125 °C
DIN 53752
 61.0 µm/m-°C
@Temperature 175 °C
DIN 53752
CTE, linear, Parallel to Flow 55.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-1/-2
 62.0 µm/m-°C
@Temperature 140 - 180 °C
ISO 11359-1/-2
Deflection Temperature at 0.46 MPa (66 psi) 212 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 196 °CISO 75-2
Glass Transition Temp, Tg 220 °CISO 11357-1/-2
Decomposition Temperature >= 400 °C
Flammability, UL94 V-0
@Thickness 1.60 mm
 V-0
@Thickness 3.20 mm
Ignition Temperature 580 - 600 °CASTM D1929
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.655
@Thickness 2.00 mm,
Wavelength 700 nm
 1.665
@Thickness 2.00 mm,
Wavelength 590 nm
 1.675
@Thickness 2.00 mm,
Wavelength 550 nm
 1.70
@Thickness 2.00 mm,
Wavelength 450 nm
 1.76
@Thickness 2.00 mm,
Wavelength 560 nm
Transmission, Visible 60 %
@Thickness 2.00 mm,
Wavelength 400 nm
 80 %
@Thickness 2.00 mm,
Wavelength 500 nm
 85 %
@Thickness 2.00 mm,
Wavelength 600 nm
UV Transmittance 3.0 %
@Thickness 2.00 mm,
Wavelength 300 nm
 30 %
@Thickness 2.00 mm,
Wavelength 350 nm
 30 %
@Thickness 2.00 mm,
Wavelength 200 nm
 
Processing PropertiesOriginal ValueComments
Melt Temperature 350 - 390 °CInjection molding
Mold Temperature 140 - 180 °CInjection molding
 
Descriptive Properties
Change in Cross Section0.1Injection-molded tensile bars after immersion in water at 23°C up to saturation
Change in Length0.1Injection-molded tensile bars after immersion in water at 23°C up to saturation
ColorColored
 Natural
Commercial StatusNorth America and Europe
Primary Processing TechniqueInjection Molding and Extrusion
Strain0.1810 hr @ 30 MPa
 0.2810 hr @ 42 MPa
 0.51 hr @ 10 MPa
 0.5110 hr @ 10 MPa
 0.52100 hr @ 10 MPa
 0.531000 hr @ 10 MPa
 1.11 hr @ 20 MPa
 1.210 hr @ 20 MPa
 1.25100 hr @ 20 MPa
 1.281000 hr @ 20 MPa
 1.751 hr @ 30 MPa
 1.95100 hr @ 30 MPa
 2.11000 hr @ 30 MPa
 2.51 hr @ 40 MPa
 2.610 hr @ 40 MPa
 2.7100 hr @ 40 MPa
 2.751 hr @ 42 MPa
 31000 hr @ 40 MPa
 3100 hr @ 42 MPa
 3.21000 hr @ 42 MPa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
BASF Ultrason® S 3010 PSU
BASF Ultrason® P 3010 MR SW 10101 PPSU
BASF Ultrason® S 2010 PSU
Ensinger RADEL® R-5500 Polyphenylsulfone (PPSU)
Overview of materials for Polyphenylsulfone (PPSU)

PBASG0169 / 131802

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.