MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Garlock GYLON® 3510 PTFE Gasketing, Barium Sulfate Filler
Categories: Polymer; Thermoplastic; Fluoropolymer; Polytetrafluoroethylene (PTFE)

Material Notes: PTFE with barium sulfate filler.
  • Improved sealing performance over conventional PTFE
  • Unique manufacturing process minimizes cold flow problems typical of skived and expanded PTFE sheets
  • Excellent bolt torque retention
  • Withstands a wide range of chemicals for extended service life
Media: Strong caustics, Moderate acids, Chlorine, Gases, Water, Steam, Hydrocarbons, Cryogenics and aluminum fluoride

Information provided by Garlock Rubber Technologies

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Permeability 0.0150.015Gas Permeability, cc/min; DIN 3535 Part 4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 13.8 MPa2000 psiacross grain; ASTM F152
 
Electrical PropertiesMetricEnglishComments
Dielectric Strength >= 18.3 kV/mm
@Temperature 121 °C,
Time 10800 sec
>= 466 kV/in
@Temperature 250 °F,
Time 3.00 hour
0.0625 in. thickness; ASTM D149
 2.32 kV/mm
@Thickness 1.59 mm
59.0 kV/in
@Thickness 0.0625 in
100% RH for 96 hours; ASTM D149
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 260 °C
@Pressure 8.27 MPa
500 °F
@Pressure 1200 psi
Continuous
Minimum Service Temperature, Air -268 °C-450 °F
 
Descriptive Properties
ColorOff-White
Compressibility, %4-10ASTM F36
Creep Relaxation, %11ASTM F38
Sealability ASTM F37B, ml/hr0.04ASTM Fuel A

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PGARL816 / 157494

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.